Tel: +86 15221953351 E-mail: info@herchyrubber.com
Please Choose Your Language
PRODUCTS
Koj tseem nyob ntawm no: Tsev » Cov khoom » Synthesis Roj Hmab » VMQ silicone » GA-57XX Kub Stamping Roller Silicone Rubber (HCR)

thauj khoom

Share rau:
facebook share khawm
twitter sib koom khawm
kab sib koom khawm
wechat sib koom khawm
linkedin sib koom khawm
pinterest sib koom khawm
whatsapp share khawm
share this share khawm

GA-57XX Kub Stamping Cov Menyuam Silicone Roj Hmab (HCR)

GA-57XX Kub stamping cov menyuam silicone roj hmab (HCR)
 
Daim ntawv thov: haum rau kev tsim kub stamping cots, kub stamping phaj, kub hloov cov menyuam, tshuab luam ntawv cov menyuam, thiab lwm yam.
 
Cov yam ntxwv tseem ceeb: kev ua haujlwm zoo heev rau qhov kub thiab txias (60 'C -350 'C), siab resilience thiab zoo abrasion tsis kam, qis deformation teeb, nyuaj rau deformation thiab tawg, lub neej ntev kev pab cuam.
  • GA-57XX UAS

  • Herchy

Muaj:
Quantity:
GA-57XX Kub stamping cov menyuam silicone roj hmab (HCR)


Daim ntawv thov: haum rau kev tsim kub stamping cots, kub stamping phaj, kub hloov cov menyuam, tshuab luam ntawv cov menyuam, thiab lwm yam.

Cov yam ntxwv tseem ceeb: kev ua haujlwm zoo heev rau qhov kub thiab txias (60 'C -350 'C), siab resilience thiab zoo abrasion tsis kam, qis deformation teeb, nyuaj rau deformation thiab tawg, lub neej ntev kev pab cuam.

Kev Ntsuas: 1% ntawm tus neeg saib xyuas (50% muab tshuaj txhuam ntawm DBPMH hauv cov pos hniav silicone), 175 'C x 5min x 15MPa.



Khoom parameters


Khoom TSI-5750 TIAB SA-5770 TIAB SA-5780 TIAB SA-5741 TIAB SA-5761
Qhov tshwm sim Hoary Fait daj
Hardness (ShoreA) 55 70 80 43 60
Tensile zog (MPa) 5.5 6 7 6 8
Elongation (%) 230 150 100 400 350
Lub zog tawg (kN / m) 10 9 9 15 25
175'C x22h Compression(%) 8 10 10 10 10


Yav dhau los: 
Tom ntej: 

QUICK LINKS

Peb cov khoom

Tiv tauj xov xwm

Ntxiv: No.33, Txoj Kev 159, Taiye Road, Fengxian District, Shanghai
Tel / WhatsApp / Skype: +86 15221953351
Copyright     2023 Shanghai Herchy Rubber Co., Ltd. Daim duab qhia chaw |   Txoj Cai Tswjfwm Ntiag Tug | Txhawb nqa By Leadong.