Gwaji: Rabo A/B na 1:1, 130°C x 5min x 15MPa
| Siffofin samfur | |||||||
| Samfura | GA-2525 | GA-2530 | GA-2540 | GA-2850 | GA-2860 | GA-2870 | |
| Bayyanar | Translucent | ||||||
| Dangantaka (Pa.s) |
80 | 80 | 80 | 220 | 300 | 400 |
|
| Hardness ( ShoreA) | 25 | 30 | 40 | 50 |
60 |
70 |
|
| Girma (g/cm3) | 1.08 | 1.10 | 1.11 | 1.13 | 1.14 |
1.16 |
|
| Ƙarfin ɗaure (MPa) | 4.5 |
5.0 |
5.5 |
6.0 |
6.0 |
5.0 |
|
| Tsawaita(%) | 400 | 350 | 300 | 250 | 220 |
180 |
|
| Ƙarfin hawaye (kN/m) | 12 | 14 | 18 |
20 | 18 |
16 |
|
| Ragewar layi (%) | 2.0 | 2.0 | 2.0 | 2.0 | 2.0 |