Nhwɛsoɔ: 0 Ɔkyerɛwfoɔ: Site Editor Bere a wɔde tintimii: 2023-08-13 Mfiase: Beaeɛ
Compression rubber dodow no ara a wɔde yɛ V-belts a ɛyɛ mpapahwekwa wɔ amannɔne aman mu no yɛ SBR/abɔde mu rɔba nipadua ne chloroprene rɔba bi. Transmission belt yɛ ahoɔden a wɔde di dwuma rɔba nneɛma, ɛsɛ sɛ formula no susuw tumi cranking adwumayɛ, ɔhyew awo ntoatoaso, kata rɔba nso ɛsɛ sɛ wobu no sɛ abrasion resistance, ɛnsɛ sɛ rɔba a ɛwɔ mu no sua dodo. Wɔde drive belts a ɛkorɔn te sɛ V-belts teateaa, kuayɛ V-belts, V-belts a wɔatwa ano, multiribbed belts ne synchronous belts di dwuma kɛse wɔ chloroprene rɔba mu. chloroprene rɔba wɔ ahoɔden kɛse, ɛko tia ɔhyew, ɛko tia onyin, ɛko tia ozone, ɛko tia abrasion, ɛbrɛ yiye wɔ flexural, na ɛbata nneɛma afoforo ho yiye. Ɔhyew a ɛfata no taa yɛ -30 ~ 100°C. Amannɔne nkitahodi abɔso dodow no ara de chloroprene rɔba a wɔde di dwuma wɔ ɔkwan a ɛkɔ akyiri so a ɛnyɛ ahwehwɛ pii na edi dwuma. Nea edidi so yi yɛ neoprene ahorow abien a wɔde dii dwuma wɔ nhwehwɛmu yi mu no adwumayɛ ho nkyerɛkyerɛmu
CR232: Saa ade yi yɛ chloroprene polymer a diisopropyl dithiocarbonate yɛ regulator. Crystallization ahoɔhare yɛ medium, density yɛ 1.23, beige lumps, ɛnyɛ efĩ. Ɛwɔ ɔhyew a ɛko tia yiye na ɛma ɔhyew a ɛkɔ soro gyina pintinn. Wobetumi de adi dwuma ama rɔba a ɛyɛ kɔla ahorow nyinaa, te sɛ nsɔano, mfutuma a wɔde kata so, rollers, lining, hose outer sheath ne rɔba afã horow afoforo. Saa ade yi te sɛ DuPont W-type ne Nidec M-40-type chloroprene rɔba.
CR322: Saa ade yi yɛ chloroprene polymer a sulphur ne diisopropyl dithiocarbonate yɛ ade a wɔde frafra na ɛsesa. Medium crystallization ahoɔhare, density 1.23, beige anaa brown akuru, a ɛnyɛ efĩ. Ahoɔden a ɛkorɔn a ɛma nusu, adwumayɛ adwumayɛ ye sen rɔba a sulfur ahyɛ so. Wobetumi de adi dwuma wɔ cable sheaths, conveyor belts ne rɔba nneɛma afoforo a wɔyɛ mu. Saa ade yi te sɛ DuPont GW type rɔba.
2.1 Nkɛntɛnso a CR ahodoɔ ne dodoɔ a wɔde ma wɔ vulcanization adwumayɛ ne Mooney viscosity a ɛwɔ V-belt compression rubber mu.
CR2322 dodow a ɛkɔ soro no, t 10, t 90 di kan yɛ tiaa na afei ɛyɛ tenten, eyi te saa efisɛ CR2322 yɛ nea ɛnyɛ sulfur-conditioned, ZnO, MgO sɛ CR2322 sulfurizing agent dosage fixed, CR2322 dodow no ne relative sulfurizing agent a ɛwɔ CR biara mu no yɛ pɛ, enti dodow no ara na ɛyɛ kɛse dodow a wɔde ma CR2322 t 10, t 90 tenten. Na M HM L nsakra pii. Bio nso, bere a CR3222 dodow kɔ soro no, t 10 ne t 90 yɛ tiaa. Eyi fi nokwasɛm a ɛyɛ sɛ CR3222 yɛ afrafra na wɔayɛ nsakrae, ZnO, MgO ne S bom yɛ adwuma sɛ vulcanizing agents, na esiane sɛ CR ankasa wɔ coking bere tiaa na ɛyɛ ntɛm sen NR/BR nti, vulcanization ahoɔhare no yɛ ntɛmntɛm bere a CR3222 dodow kɔ soro no, na M HM L no kɔ soro nkakrankakra. Awiei koraa no, wɔ mprempren vulcanization nhyehyɛe no ase no, CR3222 wɔ bere tiaa a ɛhyew, vulcanization ntɛmntɛm ne vulcanization dodow a ɛkorɔn sen CR2322.
Mooney mu ntini a ɛyɛ den no kɔɔ soro kɛse bere a CR dodow a wɔde ma no kɔɔ soro no. CR2322 kɔ soro sen CR3222 bere a CR dodow kɔ soro no, nanso CR3222 yɛ kɛse bere a wɔde CR dodow koro no ara di dwuma no.
2.2 Nsunsuansoɔ a CR ahodoɔ ne dodoɔ a wɔde ma wɔ V-belt compression rubber honam fam ne mfiridwuma mu su so
Sɛ CR2322 dodow kɔ soro a, nsakrae a ɛba wɔ tensile ahoɔden mu nyinaa nyɛ kɛse, elongation wɔ break no so tew, 100% tensile stress ne hardness no kɔ soro. Na wɔ 100 °C bere a onyin bere ntrɛwmu, tensile ahoɔden, tearing elongation so tew na pii CR2322 dosage, tensile ahoɔden, tearing elongation so tew kakraa bi; ne onyin bere ntrɛwmu 100% daa elongation, hardness kɔ soro, ne dosage soronko a CR2322, 100% daa elongation, hardness kɔɔ soro margin ketewaa bi, nanso wɔyɛ nketewa sen formula a enni CR2322.
Bere a CR3222 dodow kɔɔ soro bere a na onnyinii no, ahoɔden a ɛtwetwe no ansakra kɛse, tensile elongation no so tew, 100% constant tensile stress no so tew kan na afei ɛkɔɔ soro, na hardness no ansakra kɛse. Na wɔ 100 °C tebea a onyin bere ntrɛwmu, tensile ahoɔden, tearing elongation so tew na ɛsono dosage CR3222 tensile ahoɔden, tearing elongation so tew kakraa bi, nanso wɔyɛ nketewa sen formula a enni CR3222 ne onyin bere ntrɛwmu a 100% fixed tensile, hardness kɔ soro, na soronko dosage CR3222 100% fixed tensile, hardness nkɔanim nyɛ soronko koraa. Wɔ onyin bere soronko a CR dodow koro no ara wɔ 100 °C ase no, nsakrae a ɛba wɔ CR3222 ahoɔden a ɛtwetwe mu no sua sen CR2322 de bere a onyin bere no kyɛ; nsakrae a ɛba wɔ tearing elongation, 100% elongation, ne Shore A hardness a ɛwɔ CR3222 ne CR2322 mu no nyɛ soronko koraa wɔ CR2322 de no ho.
Wɔ mprempren sulfide nhyehyɛe no ase no, CR2322 no flexural property no ye sen CR3222 de no wɔ 80 °C, na bere a CR2322 dodow kɔ soro no, wonya flexural property a eye sen biara bere a CR2322 dodow yɛ afã horow 20, na flexural su no sɛe bere a CR3222 dodow kɔ soro no.
2.3 Mullins Nkɛntɛnso a CR ahodoɔ ne dodoɔ a wɔde di dwuma wɔ V-belt Compression Adhesives so
Esiane sɛ wɔde nhyɛso rɔba no to nhyɛso nhyɛso a wɔtaa yɛ bere a wɔde di dwuma daa no mu, na Mullins nkɛntɛnso a ɛwɔ nhyɛso ase no kyerɛ nhyɛso a ɛyɛ mmerɛw wɔ vulcanized rɔba mu wɔ nhyɛso a wɔtaa yɛ ase nti, ɛsɛ sɛ nhyɛso rɔba no nya stiffness pa wɔ cyclic compression stress ase, na ɛsɛ sɛ nhyɛso a ɛyɛ mmerɛw no yɛ ketewaa sɛnea ɛbɛyɛ yiye biara, enti wɔde Mullins nkɛntɛnso a ɛwɔ nhyɛso ase no di dwuma de kyerɛ tebea a compression rubber no adwennwen a ɛyɛ mmerɛw. V-belts a ɛyɛ mpapahwekwa no hyew a ɛfata no bɛyɛ 80 °C, enti sɛnea ɛbɛyɛ a wobetumi ayɛ sɛnea wɔde compression adhesive no di dwuma daa no ho mfonini no, wɔsɔɔ Mullins nkɛntɛnso a ɛwɔ 80 °C no hwɛe sɛnea ɛbɛyɛ a ɛbɛda tebea no a wɔde di dwuma ankasa no adi.
Sɛ CR2322 dodow kɔ soro a, ahoɔden a ɛsen biara a wɔde mia no kɔ soro ansa na 100°C × 24h anyin ne akyi. Sɛ CR2322 dodow a wɔde di dwuma no yɛ pɛ a, ahoɔden a ɛsen biara a wɔde mia no kɔ soro kɛse wɔ 100 °C × 24 h onyin akyi. Esiane sɛ nsonsonoe ketewaa a ɛda nhyɛso tumi a edi kan ne nea ɛto so abiɛsa ntam no kyerɛ sɛ Mullins nkɛntɛnso no yɛ mmerɛw nti, ɛda adi sɛ Mullins nkɛntɛnso no yɛ mmerɛw bere a CR2322 dodow kɔ soro no, na Mullins nkɛntɛnso no da so ara yɛ mmerɛw bere a CR2322 dodow a ɛkɔ soro wɔ 100 °C × 24 h akyi no. Nanso, sɛ wɔde toto nea ɛwɔ hɔ ansa na obi abɔ akwakoraa ne aberewa ho a, tumi a ɛsen biara a wɔde mia so no bo kɔ soro ansa na obi abɔ akwakoraa ne aberewa ne bere a onyin akyi. Nanso, sɛ wɔde toto nea ansa na wɔrebɔ akwakoraa ne aberewa ho a, Mullins nkɛntɛnso dodow kɔɔ soro wɔ 100 °C × 24 h onyin akyi, na Mullins nkɛntɛnso dodow a ɛkɔɔ soro no so tew bere a CR2322 dodow kɔɔ soro no.
CR3222 wɔ nhyehyɛe a ɛte saa ara ne CR2322 wɔ Mullins nkɛntɛnso ho. Ntotoe a ɛkɔ akyiri a ɛda CR3222 ne CR2322 ntam no kyerɛ sɛ wɔ tumi a ɛsen biara mu no, CR3222 sõ kɛse sen CR2322 wɔ CR dodow koro no ara mu, na saa ara na ɛte wɔ onyin akyi wɔ 100 °C × 24 h. Wɔ Mullins nkɛntɛnsoɔ no ho no, nsonsonoeɛ a ɛwɔ Mullins nkɛntɛnsoɔ mu wɔ CR3222 ne CR2322 ntam wɔ CR dodoɔ korɔ no ara mu ansa na wɔrenyin wɔ 100 °C × 24 h no nyɛ kɛseɛ, nanso nsonsonoeɛ a ɛwɔ Mullins nkɛntɛnsoɔ mu wɔ CR2322 ne CR322 ntam wɔ 100 °C × 24 h ntam no nyɛ kɛseɛ. Nanso, bere a obi anyin wɔ 100 °C × 24 h akyi no, Mullins nkɛntɛnso a ɛwɔ CR3222 mu no yɛ mmerɛw sen CR2322 de wɔ CR dodow koro no ara mu.
2.4 Nsunsuansoɔ a CR ahodoɔ ne dodoɔ ahodoɔ nya wɔ V-belt compression rubber a ɛyɛ dynamic heat generation so
Adehwere factor (tanδ), a ɛyɛ tangent a ɛwɔ phase nsonsonoe angle a ɛda strain ne stress cycle a ɛwɔ viscoelastic ade mu wɔ adeyɛ a ɛyɛ alternating force field ase no nso ne adehwere modulus no ne ahoɔden a wɔkora so modulus a ɛwɔ ade no mu no nsusuwii yɛ pɛ, na ɛyɛ index a ɛho hia a wɔde susuw ɔhyew a ɛyɛ nnam a ɛba wɔ rɔba nneɛma mu. Enti, wɔyɛɛ nkɛntɛnso a CR ahorow ne dodow ahorow nya wɔ V-belt compression rubber tanδ so no mu nhwehwɛmu.
Dodow a sɔhwɛ no hyew kɔ soro no, dodow no ara na tanδ a ɛwɔ rɔba a wɔayɛ no vulcanized no mu no kɔ fam, na dodow no ara na tanδ a ɛwɔ rɔba a wɔayɛ no vulcanized no mu kɔ soro bere a wɔde CR di dwuma no, eyi ne nokwasɛm a ɛyɛ sɛ CR wɔ Cl afã kuw wɔ ne molecule nhyehyɛe mu no wɔ abusuabɔ.
Eyi ne Cl afã kuw a ɛwɔ CR molecule nhyehyɛe mu no wɔ abusuabɔ. Rɔba a wɔde vulcanized ayɛ no tanδ so tew bere a CR2322 dodow kɔ soro no, nanso nsonsonoe no nna adi bere a ɔhyew no sua sen 100°C no. Bio nso, tanδ a ɛwɔ rɔba a wɔde vulcanized ayɛ no so tew bere a CR3222 dodow kɔ soro no, nanso nsonsonoe no nna adi wɔ nea ennu 100°C mu. Bio nso, tanδ a ɛwɔ rɔba a wɔde vulcanized ayɛ no mu no sua sen biara wɔ CR3222 no afã horow 20 mu. Wɔ ntotoho a ɛkɔ akyiri mu no, tanδ a ɛwɔ CR3222 mu no sua sen CR2322 de no wɔ ɔhyew koro no ara mu ne CR dodow koro no ara mu, a ebetumi aba sɛ efi nsonsonoe a ɛwɔ tanδ mu wɔ rɔba a wɔde sa yare no mu esiane nsonsonoe a ɛwɔ molecule nhyehyɛe ne vulcanization nhyehyɛe a wɔhwehwɛ mu wɔ ɔfã biako nti, ne nsonsonoe a ɛwɔ tanδ a ɛwɔ rɔba a wɔde sa yare no mu esiane nsonsonoe a ɛwɔ rɔba a wɔde sa yare no mu esiane nsonsonoe a ɛwɔ cross-linking density a ɛwɔ so nti ɔfã foforo no nso.
3 Awiei
(1) Bere a CR2322 a wɔde dii dwuma no kɔɔ soro no, wɔtew t 10 ne t 90 so na afei wɔtrɛw mu, na M HM L ansakra kɛse. Bere a CR3222 kɔɔ soro no, t 10 ne t 90 yɛɛ tiaa na M HM L kɔɔ soro nkakrankakra. Mooney no viscosity kɔ soro kɛse bere a CR dodow kɔ soro no, na CR2322 sõ sen CR3222 wɔ amplitude a ɛkɔ soro no mu, nanso CR3222 bo yɛ kɛse bere a wɔde CR dodow koro no ara di dwuma no.
(2) Bere a CR2322 a wɔde di dwuma no kɔ soro no, ahoɔden a ɛtwetwe no nyinaa nsakra kɛse, ahoɔden a ɛtwetwe no so tew, elongation ne hardness 100% no kɔ soro. Sɛ CR3222 kɔ soro a, ahoɔden a ɛtwetwe no nsakra pii, elongation a ɛwɔ tete mu no so tew, 100% elongation stress no so tew na afei ɛkɔ soro, na hardness no nsakra pii. CR abien no nyinaa honam fam ne mfiridwuma mu nneɛma a wɔkora so no kɔɔ soro bere a wɔanyin wɔ 100°C × 24 h akyi. Wohui sɛ mprempren vulcanization nhyehyɛe no nso wɔ honam fam ne mfiridwuma mu nneɛma a ɛkora so kɛse. Wɔ mprempren vulcanization nhyehyɛe no ase no, CR2322 a ɛko tia flexural no ye koraa sen CR3222 de wɔ 80°C.
(3) Bere a CR dodow kɔ soro no, Mullins nkɛntɛnso no so tew na tumi a ɛsen biara no kɔ soro. Wɔ ahoɔden a ɛsen biara mu no, ɛda adi sɛ CR3222 sõ sen CR2322 wɔ CR dodow koro no ara mu, na ɛte saa ara nso wɔ onyin akyi wɔ 100 °C × 24 h. Wɔ Mullins nkɛntɛnso ho no, ansa na obi nyin wɔ 100 °C × 24 h no, nsonsonoe kɛse biara nni CR3222 ne CR2322 ntam wɔ Mullins nkɛntɛnso a ɛwɔ CR dodow koro no ara mu, nanso bere a wɔanyin wɔ 100 °C × 24 h akyi no, CR3222 ne CR2322 wɔ flexural su a eye sen CR2322 wɔ CR koro no ara mu dodow a wɔde ma. Nanso, bere a obi anyin wɔ 100 °C × 24 h akyi no, Mullins nkɛntɛnso a ɛwɔ CR3222 mu no yɛ mmerɛw sen CR2322 de wɔ CR dodow koro no ara mu.
(4) Tanδ a ɛwɔ rɔba a wɔde vulcanized ayɛ no so tew bere a wɔde CR2322 di dwuma kɛse no, nanso nsonsonoe no nna adi bere a ennu 100 °C no. Bio nso, bere a CR3222 dodow kɔ soro no, tanδ a ɛwɔ rɔba a wɔde vulcanized ayɛ mu no sua sen biara bere a CR3222 dodow yɛ afã 20 no. CR3222 tanδ no sua sen CR2322 de no wɔ sɔhwɛ hyew koro no ara mu ne CR dodow koro no ara mu.