U mona: Lehae » Litaba » Tšusumetso ea limaraka tse fapaneng le litekanyetso tsa rabara Litaba ea chloroprene ts'ebetsong ea sekhomaretsi sa compression bakeng sa mabanta a V.

Tšusumetso ea limaraka tse fapaneng le litekanyetso tsa rabara ea chloroprene ts'ebetsong ea sekhomaretsi sa compression bakeng sa mabanta a V.

Maikutlo: 0     Mongoli: Nako ea Phatlalatso ea Mohlophisi oa Sebaka: 2023-08-13 Tšimoloho: Sebaka

Botsa

Boholo ba rabara e hatellang bakeng sa mabanta a V a tloaelehileng linaheng tse ling ke SBR/'mele oa rabara oa tlhaho le rabara ea chloroprene. Lebanta la phetiso ke ts'ebeliso e matla ea lihlahisoa tsa rabara, foromo e lokela ho ela hloko ts'ebetso e matla ea cranking, tlhahiso ea mocheso, rabara ea sekoaelo le eona e lokela ho nkuoa e le khanyetso ea abrasion, litaba tsa rabara ha lia lokela ho ba tlase haholo. Mabanta a maemo a holimo a kang V-mabanta a moqotetsane, V-mabanta a temo, V-mabanta a nang le maqeba a sehiloeng, mabanta a mangata le mabanta a synchronous a sebelisoa haholo ka rabara ea chloroprene. rabara ea chloroprene e na le matla a phahameng, ho hanyetsa mocheso, ho hanyetsa botsofali, ho hanyetsa ozone, ho hanyetsa abrasion, mokhathala o motle oa flexural, le ho khomarela hantle le lisebelisoa tse ling. Mocheso o sebetsang ka kakaretso ke -30 ~ 100 ℃. Mabanta a mangata a phetisetso ea kantle ho naha a sebelisa rabara ea chloroprene e tlase ea crystallinity general-purpose. Tse latelang ke li-index tsa tšebetso tsa limaraka tse peli tsa neoprene tse sebelisitsoeng phuputsong ena


CR232: Sehlahisoa sena ke chloroprene polymer e nang le diisopropyl dithiocarbonate e le molaoli. Lebelo la crystallization le mahareng, letsoalo ke 1.23, maqeba a beige, ha a silafatse. E na le ho hanyetsa mocheso o motle le botsitso bo phahameng ba mocheso. E ka sebelisoa bakeng sa mefuta eohle ea lihlahisoa tsa rabara tse mebala e khanyang, joalo ka litiiso, sekoaelo sa lerōle, li-roller, lining, sheath ea kantle ea li-hose le likarolo tse ling tse fapaneng tsa rabara. Sehlahisoa sena se tšoana le rabara ea chloroprene ea mofuta oa DuPont le Nidec's M-40-type chloroprene.


CR322: Sehlahisoa sena ke chloroprene polymer e nang le sebabole le diisopropyl dithiocarbonate e le motsoako le ho lokisa. Lebelo le bohareng la crystallization, letsoalo la 1.23, maqeba a beige kapa a sootho, a sa silafatsang. Matla a phahameng a ho tabola, ts'ebetso ea ts'ebetso e betere ho feta rabara e laoloang ke sebabole. E ka sebelisoa ha ho etsoa li-cable sheaths, mabanta a conveyor le lihlahisoa tse ling tsa rabara. Sehlahisoa sena se tšoana le rabara ea mofuta oa DuPont GW.


2.1 Tšusumetso ea limaraka tse fapaneng le litekanyetso tsa CR ts'ebetsong ea vulcanization le Mooney viscosity ea V-belt compression rabara.


Ka keketseho ea litekanyetso tsa CR2322, t 10, t 90 e khutsufatsa pele ebe ea lelefatsa, sena ke hobane CR2322 ha e na sebabole, ZnO, MgO joalo ka CR2322 sulfurizing agent dosage e tsitsitseng, CR2322 litekanyetso li lekana le CR2322 e lekanang le e 'ngoe le e' ngoe ea sulfurizing. tekanyo ea CR2322 t 10, t 90 nako e telele. Mme M HM L ha e fetohe haholo. Ho phaella moo, ha palo ea CR3222 e eketseha, t 10 le t 90 li khutšoanyane. Sena se bakoa ke taba ea hore CR3222 ke mofuta o tsoakiloeng le o fetotsoeng, ZnO, MgO le S li sebetsa hammoho e le li-agent tse senyang, 'me kaha CR ka boeona e na le nako e khutšoanyane le e potlakileng ea ho pheha ho feta NR / BR, lebelo la vulcanization le fetoha ka potlako ka keketseho ea litekanyetso tsa CR3222,' me M HM L e ntse e eketseha butle-butle. Qetellong, tlas'a tsamaiso ea hona joale ea vulcanization, CR3222 e na le nako e khutšoanyane ea ho chesa, lebelo le potlakileng la vulcanization le tekanyo e phahameng ea vulcanization ho feta CR2322.


Viscosity ea mooney e ile ea eketseha haholo ka keketseho ea litekanyetso tsa CR. CR2322 e eketsa ho feta CR3222 ka litekanyetso tse ntseng li eketseha tsa CR, empa CR3222 e kholoanyane ha palo e lekanang ea CR e sebelisoa.


2.2 Phello ea limaraka tse fapaneng le litekanyetso tsa CR ho thepa ea 'mele le ea mochini ea V-belt compression rabara


Ka keketseho ea litekanyetso tsa CR2322, phetoho e akaretsang ea matla a ho tiea ha e bohlokoa, bolelele nakong ea khefu boa fokotseha, khatello ea maikutlo le boima ba 100%. 'Me ho 100 ℃ ka nako ea botsofali katoloso, matla a tsitsipano, ho tabola elongation e fokotsehile' me tekanyo ea CR2322 e eketsehileng, matla a tsitsitseng, ho tabola elongation e fokotsehile; le nako ea botsofali katoloso ea 100% kamehla elongation, boima e ile ea eketseha, 'me fapaneng litekanyetso li behoa CR2322, 100% kamehla elongation, boima e ile ea eketseha ka margin e nyenyane, empa li nyenyane ho feta foromo ntle CR2322.


Ka keketseho ea tekanyo ea CR3222 ha e se e tsofetse, matla a ho tsitsipana ha aa ka a fetoha haholo, ho phahama ha sekhahla ho fokotsehile, khatello ea maikutlo e sa khaotseng ea 100% e ile ea fokotseha pele ebe ea eketseha, 'me boima ha boa fetoha haholo. 'Me tikolohong ea 100 ℃ e nang le katoloso ea nako ea botsofali, matla a ho tsieleha, ho hahola ho fokotseha ho fokotsehile le tekanyo e fapaneng ea matla a CR3222, ho senya elongation e fokotsehile ka chelete e nyenyane, empa e nyenyane ho feta foromo ntle le CR3222; ka katoloso ea nako ea botsofali ea 100% e tsitsitseng, ho thatafala hoa eketseha, le litekanyetso tse fapaneng tsa CR3222 tsa 100% tse tsitsitseng, ho eketseha ha boima ha ho fapane haholo. Tlas'a nako e fapaneng ea botsofali ea palo e lekanang ea CR ho 100 ℃, sekhahla sa phetoho ea matla a ho tsitsa a CR3222 e nyane ho feta ea CR2322 ka nako ea botsofali e lelefalitsoeng; sekhahla sa phetoho ea ho tabola elongation, 100% elongation, le Shore A hardness ea CR3222 le CR2322 ha li fapane haholo le tsa CR2322.


Tlas'a tsamaiso ea hona joale ea sulfide, thepa ea flexural ea CR2322 e molemo haholo ho feta ea CR3222 ho 80 ℃, 'me ha palo ea CR2322 e ntse e eketseha, thepa e ntle ka ho fetisisa ea flexural e finyelloa ha palo ea CR2322 e le likarolo tsa 20,' me thepa ea flexural e senyeha ha palo ea CR222 e eketseha.


2.3 Mullins Phello ea Mephato e fapaneng le litekanyetso tsa CR ho V-belt Compression Adhesives


Kaha rabara ea compression e tlas'a khatello ea khatello e pheta-phetoang nakong ea ts'ebeliso e tloaelehileng, 'me phello ea Mullins tlas'a khatello e bontša ho kokobetsa khatello ea kelello ea rabara e nang le vulcanized tlas'a khatello e pheta-phetoang, rabara ea compression e hloka ho ba le boima bo botle tlas'a khatello ea khatello ea kelello,' me ho nolofatsa khatello ea kelello ho lokela ho ba nyenyane ka hohle kamoo ho ka khonehang, kahoo Mullins e sebelisoa ho etsa hore khatello ea maikutlo e be tlas'a khatello ea 'mele. Mocheso o tloaelehileng oa mabanta a V a tloaelehileng a ka bang 80 ℃, kahoo e le ho etsisa tšebeliso e tloaelehileng ea sekhomaretsi sa compression, phello ea Mullins ho 80 ℃ e ile ea lekoa ho bonahatsa tšebeliso ea sebele ea mmuso.


Ka keketseho ea palo ea CR2322, matla a phahameng a khatello a eketseha pele le ka mor'a botsofali ba 100 × 24h. Ha palo ea CR2322 e sebelisitsoeng e tšoana, matla a phahameng a khatello a eketseha haholo ka mor'a ho tsofala ha 100 ℃ × 24 h. Kaha phapang e nyane pakeng tsa matla a khatello ea pele le ea boraro e bontša hore phello ea Mullins e fokola, phello ea Mullins e totobetse ka ho eketseha ha palo ea CR2322, 'me phello ea Mullins e ntse e fokola ka ho eketseha ha palo ea CR2322 ka mor'a ho tsofala ho 100 ℃ × 24 h. Leha ho le joalo, ha ho bapisoa le pele ho botsofali, matla a phahameng a khatello a eketseha pele le ka mor'a ho tsofala. Leha ho le joalo, ha ho bapisoa le pele ho botsofali, tekanyo ea phello ea Mullins e ile ea eketseha ka mor'a ho tsofala ha 100 ℃ × 24 h, 'me tekanyo ea phello ea Mullins e ile ea fokotseha ka keketseho ea litekanyetso tsa CR2322.


CR3222 e na le mokhoa o ts'oanang le CR2322 ho latela phello ea Mullins. Papiso ea longitudinal pakeng tsa CR3222 le CR2322 e bontša hore ho latela matla a mangata, CR3222 e kholo haholo ho feta CR2322 ka tekanyo e tšoanang ea CR, 'me ho joalo le ka mor'a ho tsofala ho 100 ℃ × 24 h. Mabapi le phello ea Mullins, phapang ea phello ea Mullins pakeng tsa CR3222 le CR2322 ka tekanyo e tšoanang ea CR pele e tsofala ho 100 ℃ × 24 h ha e kholo, empa phapang ea phello ea Mullins pakeng tsa CR2322 le CR322 ho 100 ℃ ha e kholo × 2 h. Leha ho le joalo, ka mor'a ho tsofala ho 100 ℃ × 24 h, phello ea Mullins ea CR3222 e fokola ho feta ea CR2322 ka tekanyo e tšoanang ea CR.


2.4 Phello ea limaraka tse fapaneng le lipalo tsa CR ho hlahisa mocheso o matla oa V-belt compression rabara


The loss factor (tanδ), e leng tangent ea angle phase ea phapang lipakeng tsa mokhahlelo le khatello ea maikutlo ea thepa ea viscoelastic tlasa ts'ebetso ea matla a chenchana, e boetse e lekana le karo-karolelano ea modulus ea tahlehelo ho modulus ea polokelo ea matla ea thepa, 'me ke index ea bohlokoa bakeng sa ho lekanya mocheso o matla oa lihlahisoa tsa rabara. Ka hona, ho ile ha fuputsoa litlamorao tsa limaraka tse fapaneng le lipalo tsa CR ho tanδ ea V-belt compression rabara.


Ha mocheso oa teko o phahame, o theola tanδ ea rabara e hlasetsoeng, 'me e phahame tanδ ea rabara e hlasetsoeng ka tšebeliso ea CR, sena se amana le taba ea hore CR e na le sehlopha sa Cl lehlakoreng sebopeho sa eona sa molek'hule.


Sena se amana le sehlopha sa lehlakore la Cl ka sebopeho sa limolek'hule tsa CR. Tanδ ea rabara e chesitsoeng e fokotseha ka ho eketseha ha palo ea CR2322, empa phapang ha e bonahale ha mocheso o le ka tlase ho 100℃. Ho feta moo, tanδ ea rabara e hlasetsoeng e fokotseha ka ho eketseha ha palo ea CR3222, empa phapang ha e bonahale ka tlase ho 100 ° C. Ho feta moo, tanδ ea rabara e chesitsoeng ke e nyane ho feta likarolo tse 20 tsa CR3222. Papisong ea longitudinal, tanδ ea CR3222 e ka tlase ho ea CR2322 ka mocheso o ts'oanang le palo e lekanang ea CR, e ka 'nang ea bakoa ke phapang ea tanδ ea rabara e phekolang ka lebaka la phapang ea sebopeho sa limolek'hule le tsamaiso e hlokahalang ea vulcanization ka lehlakoreng le leng, le ka lebaka la phapang pakeng tsa 'curingty in the rubber' ka lebaka la phapang pakeng tsa lesela le le leng. letsoho.


3 Qetello


(1) Ha tšebeliso ea CR2322 e ntse e eketseha, t 10 le t 90 li ile tsa khutsufatsoa 'me tsa lelefatsoa,' me M HM L ha ea ka ea fetoha haholo. Ka keketseho ea CR3222, t 10 le t 90 li ile tsa khutsufatsoa 'me M HM L ea eketseha butle-butle. The viscosity ea mooney e eketseha haholo ka keketseho ea tekanyo ea CR, 'me CR2322 e kholo ho feta CR3222 mabapi le ho eketseha ha amplitude, empa boleng ba CR3222 bo kholoanyane ha ho sebelisoa palo e tšoanang ea CR.


(2) Ka keketseho ea ts'ebeliso ea CR2322, matla a ho tsitsa ka kakaretso ha a fetohe haholo, matla a fokolang a fokotseha, bolelele ba 100% le boima bo eketseha. Ka keketseho ea CR3222, matla a tsitsipano ha a fetohe haholo, bolelele ba ho taboha bo fokotseha, khatello ea maikutlo ea 100% ea fokotseha ebe e ea eketseha, 'me boima ha bo fetohe haholo. Sekhahla sa ho boloka thepa ea 'mele le ea mochini oa li-CR ka bobeli e eketsehile ka mor'a botsofali ho 100 ℃ × 24 h. Tsamaiso ea hona joale ea vulcanization e ile ea boela ea fumanoa e na le tekanyo e phahameng ea ho boloka thepa ea 'mele le ea mechine. Tlas'a tsamaiso ea hona joale ea vulcanization, khanyetso ea flexural ea CR2322 e molemo haholo ho feta ea CR3222 ho 80 ℃.


(3) Ha palo ea CR e ntse e eketseha, phello ea Mullins e fokotseha 'me matla a mangata a eketseha. Mabapi le matla a mangata, ho hlakile hore CR3222 e kholo ho feta CR2322 ka tekanyo e tšoanang ea CR, hape e tšoana le ka mor'a ho tsofala ho 100 ℃ × 24 h. Mabapi le phello ea Mullins, pele botsofali ba 100 ℃ × 24 h, ha ho na phapang e ngata pakeng tsa CR3222 le CR2322 mabapi le phello ea Mullins ka tekanyo e tšoanang ea CR, empa ka mor'a ho tsofala ho 100 ℃ × 24 h, CR3222 le CR3222 le CR232 flex flex thepa e molemo haholo ho CR2322 CR2 flex tekanyo. Leha ho le joalo, ka mor'a ho tsofala ho 100 ℃ × 24 h, phello ea Mullins ea CR3222 e fokola ho feta ea CR2322 ka tekanyo e tšoanang ea CR.


(4) Tanδ ea rabara e hlasetsoeng e fokotseha ka tšebeliso e phahameng ea CR2322, empa phapang ha e bonahale ha e le ka tlase ho 100 ℃. Ntle le moo, ha palo ea CR3222 e ntse e eketseha, tanδ ea rabara e hlasetsoeng ke e nyane haholo ha palo ea CR3222 e le likarolo tse 20. Tanδ ea CR3222 e tlase ho feta ea CR2322 mochesong o tšoanang oa teko le tekanyo e tšoanang ea CR.


LIEKETSENG POTLAKO

LIHLAHISO TSA RONA

MOKHOA OA PUISANO

Eketsa: No.33, Lane 159, Taiye Road, Setereke sa Fengxian, Shanghai
Tel / WhatsApp / Skype: +86 15221953351
Copyright     2023 Shanghai Herchy Rubber Co., Ltd. Sebaka sa marang-rang |   Leano la Lekunutu | Tšehetso Ka Leadong.