Ị nọ ebe a: Ụlọ » Akụkọ » Mmetụta nke ọkwa dị iche iche na usoro nke Akụkọ chloroprene roba na arụmọrụ nke mkpakọ nrapado maka V-belts.

Mmetụta nke ọkwa dị iche iche na usoro onunu ogwu nke chloroprene rubber na arụmọrụ nke nrapado mkpakọ maka eriri V-belts.

Nlele: 0     Odee: Saịtị Editọ Oge mbipụta: 2023-08-13 Mmalite: Saịtị

Jụọ ase

Ọtụtụ n'ime rọba mkpakọ maka V-belts nkịtị na mba ọzọ bụ SBR / ahụ rọba eke na ụfọdụ roba chloroprene. Akara nnyefe bụ ihe siri ike nke ngwaahịa rọba, usoro ahụ kwesịrị iburu n'uche arụmọrụ cranking dị ike, ọgbọ okpomọkụ, mkpuchi mkpuchi kwesịrị ka a na-ewerekwa nguzogide abrasion, ọdịnaya roba ekwesịghị ịdị ala. A na-eji eriri draịva dị elu dị ka eriri V- warara, eriri V-arụ ọrụ ugbo, eriri V nwere n'ọnụ ọnụ, eriri multiribbed na eriri synchronous na-ejikarị na roba chloroprene. rọba chloroprene nwere ike dị elu, nguzogide okpomọkụ, nguzogide ịka nká, nguzogide ozone, nguzogide abrasion, ike ọgwụgwụ dị mma, yana ezigbo mmachi na ihe ndị ọzọ. The ọdabara okpomọkụ nso bụ n'ozuzu -30 ~ 100 ℃. Ọtụtụ eriri nnyefe nke mba ofesi na-eji rọba chloroprene izugbe kristal dị ala. Ndị a bụ ndepụta arụmọrụ nke akara ule abụọ nke neoprene ejiri mee ihe n'ọmụmụ ihe a


CR232: Ngwaahịa a bụ chloroprene polymer nwere diisopropyl dithiocarbonate dị ka onye na-achịkwa. Ọsọ kristal bụ ọkara, njupụta bụ 1.23, lumps beige, anaghị emetọ ya. Ọ nwere ezigbo nguzogide okpomọkụ na nkwụsi ike dị elu. Enwere ike iji ya maka ngwaahịa rọba na-acha ọkụ ọ bụla, dị ka akara, mkpuchi uzuzu, rollers, lining, sooks mpụta n'ọbọ na akụkụ roba ndị ọzọ dị iche iche. Ngwaahịa a yiri ụdị DuPont's W na Nidec's M-40-ụdị chloroprene roba.


CR322: Ngwaahịa a bụ polymer chloroprene nwere sọlfọ na diisopropyl dithiocarbonate dị ka onye na-agwakọta na nhazi. Ọsọ kristal dị ọkara, njupụta 1.23, beige ma ọ bụ akpụ aja aja, anaghị emetọ ya. Ike akwa akwa, nhazi nhazi dị mma karịa rọba na-achịkwa sọlfọ. Enwere ike iji ya na-emepụta ihe mkpuchi eriri, eriri ebu na ngwaahịa roba ndị ọzọ. Ngwaahịa a yiri DuPont GW ụdị roba.


2.1 Mmetụta nke ọkwa dị iche iche na usoro CR na arụmọrụ vulcanization na Mooney viscosity nke V-belt compression roba.


Na-abawanye nke CR2322 onunu ogwu, t 10, t 90 mbụ mkpirisi wee gbatịa, nke a bụ n'ihi na CR2322 bụ na-abụghị sọlfọ-conditioned, ZnO, MgO dị ka CR2322 sulfurizing gị n'ụlọnga usoro onunu ogwu ofu, CR2322 onunu ogwu bụ Ẹkot onye ikwu sulfurizing onye ọ bụla n'ụlọnga na-erughị ndị ikwu sulfurizing. CR2322 t 10, t 90 ogologo. Na M HM L anaghị agbanwe nke ukwuu. Na mgbakwunye, ka ọnụ ọgụgụ nke CR3222 na-abawanye, t 10 na t 90 dị mkpụmkpụ. Nke a bụ n'ihi n'eziokwu na CR3222 bụ ụdị agwakọta na gbanwee, ZnO, MgO na S na-arụkọ ọrụ ọnụ dị ka ndị na-eme ihe ike, na n'ihi na CR n'onwe ya nwere oge coking dị mkpụmkpụ na ngwa ngwa karịa NR / BR, ngwa ngwa ngwa ngwa na-abawanye na ọnụọgụ nke CR3222, na M HM L na-eji nwayọọ nwayọọ na-abawanye. N'ikpeazụ, n'okpuru usoro vulcanization dị ugbu a, CR3222 nwere oge ọkụ dị mkpụmkpụ, ọnụ ọgụgụ ngwa ngwa ngwa ngwa na ọkwa dị elu nke vulcanization karịa CR2322.


Viscosity nke Mooney mụbara nke ukwuu site na mmụba nke usoro onunu ogwu CR. CR2322 na-abawanye karịa CR3222 na-abawanye CR doses, ma CR3222 dị ukwuu mgbe a na-eji otu ego nke CR.


2.2 Mmetụta nke ọkwa dị iche iche na usoro ọgwụgwọ CR na anụ ahụ na akụrụngwa nke V-belt compression roba.


Site na mmụba nke usoro onunu ogwu CR2322, mgbanwe n'ozuzu nke ike ike adịghị mkpa, elongation na nkwụsịtụ na-ebelata, 100% nrụgide nrụgide na ike siri ike na-abawanye. Na na 100 ℃ na ịka nká oge ndọtị, ike mgbaka, tering elongation belatara na ndị ọzọ CR2322 onunu ogwu, ike ike, tering elongation ebelata obere; na oge ịka nká nke 100% elongation na-adịgide adịgide, isi ike na-abawanye, na usoro ọgwụgwọ dị iche iche nke CR2322, 100% elongation na-adịgide adịgide, ịdị ike na-abawanye site na obere oke, ma dị ntakịrị karịa usoro na-enweghị CR2322.


Site na mmụba nke usoro ọgwụgwọ CR3222 mgbe ọ na-etoliteghị, ike ike adịghị agbanwe agbanwe nke ukwuu, elongation tensile na-ebelata, 100% nrụgide na-adịgide adịgide na-ebelata na mbụ wee mụbaa, na ike adịghị agbanwe agbanwe. Na na 100 ℃ gburugburu ebe obibi na ịka nká oge ndọtị, ike ike, tering elongation belatara na dị iche iche onunu ogwu nke CR3222 tensile ike, tearing elongation belatara site a obere ego, ma ndị nta karịa usoro enweghị CR3222; na mgbatị oge ịka nká nke 100% na-edozi ahụ, a na-abawanye ike siri ike, na usoro dị iche iche nke CR3222 nke 100% na-edozi ahụ, mmụba siri ike adịghị iche. N'okpuru dị iche iche ịka nká oge nke otu ego nke CR na 100 ℃, mgbanwe ọnụego nke tensile ike nke CR3222 bụ obere karịa nke CR2322 na ịka nká oge ogologo; mgbanwe mgbanwe nke tering elongation, 100% elongation, na Shore A siri ike nke CR3222 na CR2322 adịghị nnọọ iche na nke CR2322.


N'okpuru usoro sulfide dị ugbu a, ihe na-agbanwe agbanwe nke CR2322 dị mma karịa nke CR3222 na 80 ℃, na ka ọnụ ọgụgụ nke CR2322 na-abawanye, a na-enweta ihe kacha mma na-agbanwe agbanwe mgbe ego nke CR2322 bụ akụkụ 20, na ihe na-agbanwe agbanwe na-abawanye ka ọnụ ọgụgụ nke CR32 na-abawanye.


2.3 Mmetụta Mullins nke ọkwa dị iche iche yana usoro CR na eriri mkpakọ V-belt.


Ebe ọ bụ na roba mkpakọ na-edobe nrụgide mkpakọ ugboro ugboro n'oge a na-eji ya eme ihe, na mmetụta Mullins n'okpuru mkpakọ na-egosipụta nrụgide nro nke rọba vulcanized n'okpuru mkpakọ ugboro ugboro, rọba mkpakọ kwesịrị inwe ezigbo isi ike n'okpuru nrụgide nrụgide cyclic, na nrụgide nrụgide kwesịrị ịdị ntakịrị dị ka o kwere mee, ya mere mmetụta Mullins n'okpuru mkpakọ nke mkpakọ na-eji agwa agwa. The nkịtị okpomọkụ nke nkịtị V-belts bụ banyere 80 ℃, ya mere, iji simulate nkịtị ojiji nke mkpakọ nrapado, Mullins mmetụta na 80 ℃ a nwalere na-egosipụta n'ezie ojiji nke steeti.


Na mmụba nke ego nke CR2322, kacha mkpakọ ike na-abawanye tupu na mgbe 100 ℃ × 24h ịka nká. Mgbe ọnụọgụ CR2322 ejiri mee otu ihe ahụ, ike mkpakọ kachasị na-abawanye nke ukwuu mgbe 100 ℃ × 24 h mere agadi. Ebe ọ bụ na obere ọdịiche dị n'etiti ndị agha mkpakọ nke mbụ na nke atọ na-egosi na mmetụta Mullins na-esiwanye ike, mmetụta Mullins na-esiwanye ike na mmụba nke CR2322, na mmetụta Mullins ka na-ebelata na mmụba nke CR2322 mgbe ịka nká na 100 ℃ × 24 h. Otú ọ dị, e jiri ya tụnyere nke ahụ tupu ịka nká, uru ike mkpakọ kachasị na-abawanye tupu na mgbe ịka nká gasịrị. Otú ọ dị, e jiri ya tụnyere nke ahụ tupu ịka nká, ogo nke mmetụta Mullins mụbara mgbe 100 ℃ × 24 h ịka nká, na ogo nke Mullins mmetụta mụbara na-abawanye na CR2322 onunu ogwu.


CR3222 nwere ụkpụrụ yiri ya na CR2322 n'ihe gbasara mmetụta Mullins. Ntụle ogologo dị n'etiti CR3222 na CR2322 na-egosi na n'ihe gbasara ike kachasị, CR3222 dị ukwuu karịa CR2322 n'otu usoro CR, na otu ihe ahụ bụ eziokwu mgbe ịka nká na 100 ℃ × 24 h. N'ihe gbasara mmetụta Mullins, ọdịiche dị na mmetụta Mullins dị n'etiti CR3222 na CR2322 n'otu usoro CR tupu ịka nká na 100 ℃ × 24 h adịghị mma, ma ọdịiche dị na mmetụta Mullins n'etiti CR2322 na CR322 na 100 ℃ × 24 h adịghị mma. Agbanyeghị, mgbe ịkachara ahụ na 100 ℃ × 24 h, mmetụta Mullins nke CR3222 adịghị ike karịa nke CR2322 n'otu usoro ọgwụgwọ CR.


2.4 Mmetụta nke ọkwa dị iche iche na ọnụọgụ CR na ọgbọ okpomọkụ dị ike nke V-belt compression roba


Ihe na-efunahụ (tanδ), nke bụ tangent nke akụkụ dị iche nke akụkụ dị n'etiti eriri na nrụgide nrụgide nke ihe viscoelastic n'okpuru ọrụ nke mpaghara ike ọzọ, bụkwa nha nha nke modul ọnwụ na nchekwa nchekwa ike nke ihe ahụ, ọ bụkwa ihe dị mkpa maka ịlele ọgbọ okpomọkụ dị ike nke ngwaahịa roba. Ya mere, a na-enyocha mmetụta nke ọkwa dị iche iche na ọnụọgụ CR na tanδ nke V-belt compression roba.


N'ihe dị elu nke ule nyocha, na-ebelata tanδ nke rọba vulcanized, na elu tanδ nke rọba vulcanized na iji CR, nke a metụtara eziokwu ahụ bụ na CR nwere otu akụkụ Cl n'usoro ihe omimi ya.


Nke a metụtara otu akụkụ Cl n'ime usoro ihe omimi nke CR. Tanδ nke rọba vulcanized na-ebelata site n'ịba ụba nke CR2322, mana ọdịiche ahụ apụtaghị ìhè mgbe okpomọkụ dị ala karịa 100 ℃. Na mgbakwunye, tanδ nke rọba vulcanized na-ebelata site n'ịba ụba nke CR3222, mana ọdịiche ahụ apụtaghị na ihe na-erughị 100 Celsius. Ọzọkwa, tanδ nke rọba vulcanized bụ nke kacha nta na akụkụ 20 nke CR3222. Na longitudinal ntụnyere, na tanδ nke CR3222 dị ala karịa nke CR2322 na otu okpomọkụ na otu ego nke CR, nke nwere ike ịbụ n'ihi na ihe dị iche na tanδ nke na-agwọ roba n'ihi na ihe dị iche na molekụla Ọdịdị na chọrọ vulcanization usoro n'otu aka, na n'ihi ọdịiche dị na tanδ nke ọgwụgwọ dị iche na cross-n'ihi njikọ nke ọzọ na-njikọ.


3 Nkwubi okwu


(1) Ka ojiji nke CR2322 na-abawanye, t 10 na t 90 dị mkpụmkpụ wee gbasaa ogologo oge, na M HM L agbanwebeghị nke ukwuu. Site na mmụba nke CR3222, t 10 na t 90 dị mkpụmkpụ na M HM L ji nwayọọ nwayọọ na-abawanye. Viscosity nke Mooney na-abawanye nke ukwuu site na mmụba nke usoro onunu ogwu CR, na CR2322 buru ibu karịa CR3222 n'ihe gbasara mmụba njupụta, mana uru CR3222 na-ebuwanye ibu mgbe ejiri otu ego CR.


(2) Site na mmụba nke ojiji nke CR2322, ike nkwụsị n'ozuzu adịghị agbanwe nke ukwuu, ike nkwụsị na-ebelata, 100% elongation na hardness na-abawanye. Site na mmụba nke CR3222, ike nkwụsị ahụ adịghị agbanwe nke ukwuu, elongation na dọka mmiri na-ebelata, nrụgide elongation 100% na-ebelata ma na-abawanye, na ike adịghị agbanwe nke ukwuu. Ọnụego njide nke anụ ahụ na akụrụngwa nke ma CRs mụbara mgbe ịkachara na 100 ℃ × 24 h. Achọpụtakwara sistemu vulcanization nke dị ugbu a ka ọ nwere nnukwu njide nke ihe anụ ahụ na igwe. N'okpuru usoro vulcanization dị ugbu a, nguzogide mgbanwe nke CR2322 dị mma karịa nke CR3222 na 80 ℃.


(3) Ka ọnụ ọgụgụ CR na-abawanye, mmetụta Mullins na-ebelata na ike kachasị elu na-abawanye. N'ihe gbasara ike kachasị, CR3222 doro anya karịa CR2322 n'otu usoro ọgwụgwọ CR, ọ bụkwa otu ihe ahụ mgbe ịka nká na 100 ℃ × 24 h. N'ihe banyere mmetụta Mullins, tupu ịka nká na 100 ℃ × 24 h, ọ dịghị ihe dị iche n'etiti CR3222 na CR2322 n'ihe banyere mmetụta Mullins n'otu usoro ọgwụgwọ CR, ma mgbe ịka nká na 100 ℃ × 24 h, CR3222 na CR2322 nwere ihe dị mma karịa flex CR2322 na flex. Agbanyeghị, mgbe ịkachara ahụ na 100 ℃ × 24 h, mmetụta Mullins nke CR3222 adịghị ike karịa nke CR2322 n'otu usoro ọgwụgwọ CR.


(4) Tanδ nke rọba vulcanized na-ebelata site na iji CR2322 dị elu, mana ọdịiche ahụ apụtaghị ìhè mgbe ọ na-erughị 100 ℃. Na mgbakwunye, ka ọnụ ọgụgụ nke CR3222 na-abawanye, tanδ nke roba vulcanized bụ nke kacha nta mgbe ọnụọgụ CR3222 bụ akụkụ 20. Tanδ nke CR3222 dị ala karịa nke CR2322 n'otu ọnọdụ nnwale ahụ yana otu usoro ọgwụgwọ CR.


Njikọ ngwa ngwa

Ngwaahịa anyị

OZI MKPỌTỤRỤ

Tinye: No.33, Lane 159, Taiye Road, Fengxian District, Shanghai
Tel / WhatsApp / Skype: +86 15221953351
Nwebiisinka     2023 Shanghai Herchy Rubber Co., Ltd. map saịtị |   Amụma nzuzo | Nkwado Site Leadong.