Ra'ayoyi: 0     Mawallafi: Lokacin Buga Editan Yanar Gizo: 2023-08-13 Asalin: Shafin

Tambaya

Mafi yawan robar matsawa ga talakawa V-belts a kasashen waje shine SBR/jikin roba na halitta da wasu roba na chloroprene. Belin watsawa shine amfani mai ƙarfi na samfuran roba, dabarar yakamata tayi la'akari da aikin cranking mai ƙarfi, ƙirar zafi, murfin roba kuma yakamata a yi la'akari da juriya abrasion, abun ciki na roba kada yayi ƙasa da ƙasa. Babban bel ɗin tuƙi irin su kunkuntar V-belts, V-belts na noma, V-belts tare da yanke gefuna, bel ɗin multiribbed da bel ɗin daidaitawa ana amfani da su sosai a cikin roba na chloroprene. chloroprene roba yana da ƙarfi mai ƙarfi, juriya na zafi, juriya na tsufa, juriya na ozone, juriya na abrasion, gajiya mai kyau, da mannewa mai kyau tare da sauran kayan. Matsakaicin zafin jiki mai dacewa shine gabaɗaya -30 ~ 100 ℃. Yawancin bel ɗin watsawa na ƙasashen waje suna amfani da ƙananan kristal-manufa chloroprene roba. Wadannan su ne ma'auni na aiki na maki biyu na neoprene da aka yi amfani da su a cikin wannan binciken


CR232: Wannan samfurin shine chloroprene polymer tare da diisopropyl dithiocarbonate a matsayin mai gudanarwa. Gudun crystallization yana da matsakaici, yawa shine 1.23, lumps beige, mara gurɓatacce. Yana da kyakkyawan juriya na zafi da kwanciyar hankali mai zafi. Ana iya amfani da shi don kowane nau'in samfuran roba masu launin haske, kamar hatimi, murfin ƙura, rollers, ruɗi, bututu na waje da sauran sassa daban-daban na roba. Wannan samfurin yayi kama da nau'in W-type na DuPont da nau'in chloroprene na Nidec na M-40.


CR322: Wannan samfurin shine chloroprene polymer tare da sulfur da diisopropyl dithiocarbonate a matsayin wakili mai haɗawa da daidaitawa. Matsakaici gudun crystallization, yawa 1.23, m ko launin ruwan kasa lumps, mara gurbatawa. Babban ƙarfin hawaye, aikin sarrafawa ya fi sulfur-kayyade roba. Ana iya amfani da shi wajen kera kumfa na USB, bel na jigilar kaya da sauran kayayyakin roba. Wannan samfurin yayi kama da DuPont GW nau'in roba.


2.1 Tasirin maki daban-daban da adadin CR akan aikin vulcanization da Mooney danko na V-belt compression roba.


Tare da karuwa na CR2322 sashi, t 10, t 90 na farko gajarta sa'an nan kuma tsawaita, wannan shi ne saboda CR2322 ne ba sulfur-kwandishan, ZnO, MgO kamar yadda CR2322 sulfurizing wakili sashi gyarawa, CR2322 sashi ne daidai da dangi sulfuring haka, da mafi girma wakili na kowane CR2322 dosage. CR2322 t 10, t 90 ya fi tsayi. Kuma M HM L baya canzawa sosai. Bugu da ƙari, yayin da adadin CR3222 ya karu, t 10 da t 90 sun fi guntu. Wannan shi ne saboda gaskiyar cewa CR3222 wani nau'i ne mai gauraye da daidaitawa, ZnO, MgO da S suna aiki tare a matsayin wakilai masu lalata, kuma saboda CR kanta yana da gajeren lokaci da sauri fiye da NR / BR, saurin vulcanization ya zama sauri tare da karuwa a cikin sashi na CR3222, kuma M HM L yana karuwa a hankali. A ƙarshe, a ƙarƙashin tsarin vulcanization na yanzu, CR3222 yana da ɗan gajeren lokacin ƙonawa, saurin vulcanization da mafi girman matakin vulcanization fiye da CR2322.


Dankowar Mooney ya karu sosai tare da karuwar adadin CR. CR2322 yana ƙaruwa fiye da CR3222 tare da ƙara yawan adadin CR, amma CR3222 ya fi girma idan aka yi amfani da adadin CR iri ɗaya.


2.2 Tasirin maki daban-daban da sashi na CR akan kayan aikin jiki da na injiniya na V-belt compression roba


Tare da karuwa na CR2322 sashi, gabaɗayan canjin ƙarfin ƙarfi ba shi da mahimmanci, haɓakawa a hutu yana raguwa, 100% damuwa mai ƙarfi da ƙarfin ƙarfi. Kuma a 100 ℃ tare da tsawo lokaci tsawo, tensile ƙarfi, tearing elongation rage da kuma mafi CR2322 sashi, tensile ƙarfi, tearing elongation rage kasa; tare da tsawo lokaci tsawo na 100% m elongation, taurin ya karu, da kuma daban-daban sashi na CR2322, 100% m elongation, taurin ya karu da wani karamin gefe, amma su ne karami fiye da dabara ba tare da CR2322.


Tare da karuwa na CR3222 sashi lokacin da ba a tsufa ba, ƙarfin daɗaɗɗa bai canza da yawa ba, haɓakar haɓakar haɓaka ya ragu, 100% na yau da kullun na damuwa ya ragu da farko sannan ya karu, kuma taurin bai canza ba. Kuma a 100 ℃ yanayi tare da tsufa lokaci tsawo, tensile ƙarfi, tearing elongation rage da kuma daban-daban sashi na CR3222 tensile ƙarfi, tearing elongation rage da wani karamin adadin, amma su ne karami fiye da dabara ba tare da CR3222; tare da tsawan lokacin tsufa na 100% kafaffen ƙayyadaddun ƙayyadaddun ƙayyadaddun ƙayyadaddun ƙayyadaddun ƙayyadaddun ƙayyadaddun ƙayyadaddun ƙayyadaddun ƙayyadaddun ƙayyadaddun ƙarfi, kuma nau'i daban-daban na CR3222 na 100% kafaffen ƙayyadaddun ƙayyadaddun ƙayyadaddun ƙayyadaddun ƙayyadaddun ƙarfi ba su bambanta ba. A karkashin daban-daban tsufa lokaci na daidai adadin CR a 100 ℃, da canji kudi na tensile ƙarfi na CR3222 ne karami fiye da na CR2322 tare da tsufa tsawon lokaci; canjin canjin tsaga elongation, 100% elongation, da Shore A taurin CR3222 da CR2322 ba su da bambanci da na CR2322.


A karkashin tsarin sulfide na yanzu, kayan gyare-gyare na CR2322 yana da kyau fiye da na CR3222 a 80 ℃, kuma yayin da adadin CR2322 ya karu, ana samun mafi kyawun kayan aiki lokacin da adadin CR2322 ya kasance kashi 20, kuma dukiyar da ke da alaƙa ta lalace yayin da adadin 232 ya karu.


2.3 Mullins Tasirin Maki Daban Daban da Matsaloli na CR akan Adhesives na V-belt Compression


Tun da matsawa roba aka hõre da maimaita matsawa danniya a lokacin da al'ada amfani, da kuma Mullins sakamako a karkashin matsawa halin da danniya laushi na vulcanized roba a karkashin maimaita matsawa, da matsawa roba bukatar samun mai kyau stiffness a karkashin cyclic matsawa danniya, da kuma danniya laushi ya kamata a matsayin kadan kamar yadda zai yiwu, don haka da Mullins sakamako a karkashin matsawa da ake amfani da su shafa halin danniya. A al'ada zazzabi na talakawa V-bels ne game da 80 ℃, don haka domin a kwaikwayi na al'ada amfani da matsawa m, Mullins sakamako a 80 ℃ aka gwada don nuna ainihin amfani da jihar.


Tare da karuwa na adadin CR2322, matsakaicin ƙarfin matsawa yana ƙaruwa kafin da kuma bayan 100 ℃ × 24h tsufa. Lokacin da adadin CR2322 da aka yi amfani da shi iri ɗaya ne, matsakaicin ƙarfin matsawa yana ƙaruwa sosai bayan 100 ℃ × 24 h tsufa. Tun da ƙaramin bambance-bambance tsakanin sojojin matsawa na farko da na uku yana nuna cewa tasirin Mullins ya fi rauni, tasirin Mullins yana da rauni a fili tare da haɓaka adadin CR2322, kuma tasirin Mullins har yanzu yana raunana tare da haɓakar adadin CR2322 bayan tsufa a 100 ℃ × 24 h. Koyaya, idan aka kwatanta da wancan kafin tsufa, matsakaicin ƙimar ƙarfin matsawa yana ƙaruwa kafin da bayan tsufa. Koyaya, idan aka kwatanta da wancan kafin tsufa, matakin tasirin Mullins ya karu bayan tsufa 100 ℃ × 24 h, kuma matakin tasirin Mullins ya karu tare da karuwar adadin CR2322.


CR3222 yana da irin wannan tsari tare da CR2322 dangane da tasirin Mullins. Kwatancen tsayin daka tsakanin CR3222 da CR2322 yana nuna cewa dangane da matsakaicin ƙarfi, CR3222 ya fi girma fiye da CR2322 a daidai adadin CR guda ɗaya, kuma daidai yake bayan tsufa a 100 ℃ × 24 h. Dangane da tasirin Mullins, bambancin tasirin Mullins tsakanin CR3222 da CR2322 a daidai adadin CR kafin tsufa a 100 ℃ × 24 h ba mai girma ba ne, amma bambancin tasirin Mullins tsakanin CR2322 da CR322 a 100 ℃ 24 h ba mai girma bane. Koyaya, bayan tsufa a 100 ℃ × 24 h, tasirin Mullins na CR3222 ya fi rauni fiye da na CR2322 a daidai adadin CR.


2.4 Tasirin maki daban-daban da adadin CR akan haɓakar zafi mai ƙarfi na V-belt compression roba


Matsakaicin hasara (tanδ), wanda shine tangent na kusurwar bambancin lokaci tsakanin nau'i da sake zagayowar damuwa na kayan viscoelastic a ƙarƙashin aikin madaidaicin filin ƙarfi, shima daidai yake da rabon ma'aunin asara zuwa yanayin ajiyar makamashi na kayan, kuma yana da mahimmancin ma'auni don auna ƙarfin haɓakar zafi na samfuran roba. Sabili da haka, an bincika tasirin maki daban-daban da adadin CR akan tanδ na V-belt compression roba.


Mafi girman zafin gwajin, ƙananan tanδ na roba mai ɓarna, kuma mafi girman tanδ na roba mai lalacewa tare da amfani da CR, wannan yana da alaƙa da gaskiyar cewa CR yana da ƙungiyar Cl a cikin tsarinsa na kwayoyin halitta.


Wannan yana da alaƙa da ƙungiyar gefen Cl a cikin tsarin kwayoyin halitta na CR. Tanδ na roba vulcanized yana raguwa tare da ƙara adadin CR2322, amma bambancin ba a bayyane yake ba lokacin da zafin jiki ya kasa 100 ℃. Bugu da ƙari, tanδ na roba mai ɓarna yana raguwa tare da ƙara adadin CR3222, amma bambancin ba a bayyane yake ba a ƙasa da 100 ° C. Haka kuma, tanδ na roba mai ɓarna shine mafi ƙanƙanta a sassa 20 na CR3222. A cikin kwatancen tsayin daka, tanδ na CR3222 yana ƙasa da na CR2322 a cikin zafin jiki iri ɗaya da adadin CR, wanda zai iya zama saboda bambancin tanδ na roba na curing saboda bambancin tsarin kwayoyin halitta da tsarin vulcanization da ake buƙata a hannu ɗaya, kuma saboda bambancin tanδ na bambancin curing a cikin roba-sakamakon haɗin gwiwa.


3 Kammalawa


(1) Yayin da amfani da CR2322 ya karu, t 10 da t 90 sun ragu sannan kuma sun kara tsawo, kuma M HM L bai canza ba. Tare da karuwa na CR3222, t 10 da t 90 an rage su kuma M HM L ya karu a hankali. Dankowar Mooney yana ƙaruwa sosai tare da karuwar adadin CR, kuma CR2322 ya fi CR3222 girma dangane da haɓaka girma, amma ƙimar CR3222 ya fi girma idan aka yi amfani da adadin CR iri ɗaya.


(2) Tare da karuwa a cikin yin amfani da CR2322, ƙarfin juzu'i na gaba ɗaya baya canzawa da yawa, ƙarfin ƙarfi ya ragu, 100% elongation da taurin haɓaka. Tare da haɓakar CR3222, ƙarfin ƙarfi ba ya canzawa da yawa, haɓakar haɓakar hawaye yana raguwa, 100% haɓaka damuwa yana raguwa sannan kuma yana ƙaruwa, kuma taurin baya canzawa da yawa. Adadin riƙewa na kayan aikin jiki da na injiniya na duka CRs sun ƙaru bayan tsufa a 100 ℃ × 24 h. Hakanan an gano tsarin vulcanization na yanzu yana da ƙimar riƙewa na zahiri da na inji. A karkashin tsarin vulcanization na yanzu, juriya mai juriya na CR2322 ya fi na CR3222 a 80 ℃.


(3) Yayin da adadin CR ya karu, tasirin Mullins yana raguwa kuma iyakar ƙarfin yana ƙaruwa. Dangane da matsakaicin ƙarfi, CR3222 a fili ya fi CR2322 girma a daidai adadin CR, kuma iri ɗaya ne bayan tsufa a 100 ℃ × 24 h. Dangane da tasirin Mullins, kafin tsufa a 100 ℃ × 24 h, babu bambanci sosai tsakanin CR3222 da CR2322 dangane da tasirin Mullins a cikin nau'in CR iri ɗaya, amma bayan tsufa a 100 ℃ × 24 h, CR3222 da CR2322 suna da kyawawan kaddarorin 2 fiye da flex CR2322 fiye da flex. Koyaya, bayan tsufa a 100 ℃ × 24 h, tasirin Mullins na CR3222 ya fi rauni fiye da na CR2322 a daidai adadin CR.


(4) Tanδ na roba mai ɓarna yana raguwa tare da mafi girman amfani da CR2322, amma bambancin ba a bayyane yake ba lokacin da bai wuce 100 ℃ ba. Bugu da ƙari, yayin da adadin CR3222 ya karu, tanδ na roba mai lalacewa shine mafi ƙanƙanta lokacin da adadin CR3222 shine sassa 20. Tanδ na CR3222 ya yi ƙasa da na CR2322 a zazzabin gwaji iri ɗaya da nau'in CR iri ɗaya.


SAUKAR HANYA

KAYANMU

BAYANIN HULDA

Ƙara: No.33, Lane 159, Taiye Road, Fengxian District, Shanghai
Tel / WhatsApp / Skype: +86 15221953351
Haƙƙin mallaka     2023 Shanghai Herchy Rubber Co., Ltd. Taswirar yanar gizo |   Manufar Keɓantawa | Taimako Ta Leadong.