Views: 0 Author: Site Editor Bɔli waati: 2023-08-13 Bɔyɔrɔ: Yɔrɔ
V-belt gansanw ka compression rubber fanba ye jamana wɛrɛw la, o ye SBR/natural rubber body ye ani chloroprene rubber dɔw. Transmission belt ye baarakɛcogo barikama ye lastikuw fɛ, formula ka kan ka jateminɛ kɛ dinamikɛ cranking baarakɛcogo la, funteni bɔli, datugulan lastikuw fana ka kan ka jate abrasion resistance ye, lastikuw kɔnɔfɛnw man kan ka dɔgɔya kojugu. Bololabaarakɛlaw ka cɛsirilan minnu ka bon kosɛbɛ i n’a fɔ V-belt fitininw, sɛnɛfɛnw V-beltw, V-belts minnu da tigɛlen don, multiribbed belts ani synchronous belts, olu bɛ kɛ ka caya kuloropɛrɛni lastikuw la. kuloropɛrɛni lastikuw fanga ka bon, a bɛ funteni kɛlɛ, a tɛ kɔrɔbaya, a tɛ se ka ozɔni kɛlɛ, a bɛ se ka sɔgɔsɔgɔ, a bɛ sɛgɛn ka ɲɛ, wa a bɛ nɔrɔ fɛn wɛrɛw la ka ɲɛ. A ka c’a la, funteni hakɛ min bɛ Se ka Kɛ o ye -30~100°C ye. Dunanw ka fɛnw cili cɛsirilan fanba bɛ baara kɛ ni kuloropɛrɛni lamini ye min ka kristali ka dɔgɔn. Ninnu ye neoprene suguya fila minnu kɛra nin kalan in kɔnɔ, olu ka baarakɛcogo jiralanw ye
CR232 : Nin fura in ye kuloropɛrɛni polimɛri ye min diisoporopili ditiyokarbonati ye a ɲɛnabɔbaga ye. Kristali teliya ye cɛmancɛ ye, a density ye 1,23 ye, kurukuru beige, nɔgɔ tɛ. A bɛ funteni kunbɛn koɲuman ani a bɛ sabati funteni caman na. A bɛ se ka kɛ lastikuw suguya bɛɛ la minnu ɲɛ ye jɛman ye, i n’a fɔ sigilanw, buguri datugulan, wuluwuluw, finimugu, hose kɛnɛma dawolo ani lastikuw yɔrɔ suguya wɛrɛw. Nin fura in ni DuPont ka W suguya ani Nidec ka M-40 suguya kuloropɛrɛni lastikuw bɔlen don ɲɔgɔn fɛ.
CR322 : Nin fura in ye kuloropɛrɛni polimɛri ye min kɔnɔ kisɛ ni diisoporopili ditiyokarbonati ye ɲagami ni ladilanfɛn ye. Kristali teliya cɛmancɛ, density 1,23, kurukuru beige walima bulama, nɔgɔ tɛ. Ɲɛjibɔ fanga ka bon, baarakɛcogo ɲuman ka fisa ni lastikuw ye minnu bɛ labɛn ni kisɛ ye. A bɛ se ka kɛ kabali dawolo, fɛnw lasecogo ani lastikuw wɛrɛw dilanni na. Nin fura in ni DuPont GW suguya lastikuw bɛ tali kɛ ɲɔgɔn na.
2.1 CR hakɛw ni a tata hakɛ danfaralenw nɔ min bɛ V-belt compression rubber ka vulcanization baarakɛcogo la ani Mooney viscosity la.
Ni CR2322 hakɛ cayara, t 10, t 90 bɛ fɔlɔ ka surunya ka sɔrɔ ka janya, o bɛ kɛ barisa CR2322 tɛ kisɛkisɛ la, ZnO, MgO i n’a fɔ CR2322 kisɛkisɛ hakɛ latigɛlen don, CR2322 hakɛ bɛ bɛn CR kelen-kelen bɛɛ ka kisɛkisɛ hakɛ danfaralen ma, o la, a ka bon CR2322 hakɛ t 10, t 90 ka jan. Wa M HM L tɛ Changé kosɛbɛ. Ka fara o kan, ni CR3222 hakɛ bɛ caya, t 10 ni t 90 bɛ surunya. O bɛ bɔ CR3222 suguya ɲagaminen ni ladilanni na, ZnO, MgO ani S bɛ baara kɛ ɲɔgɔn fɛ i n’a fɔ vulkanizelanw, wa ikomi CR yɛrɛ ka coke waati ka surun ani a ka teliya ka tɛmɛ NR/BR kan, vulcanization teliya bɛ teliya ni CR3222 hakɛ cayara, wa M HM L bɛ bonya dɔɔni dɔɔni. A laban na, sisan vulkanizasiyɔn siratigɛ la, CR3222 jeni waati ka surun, a vulkanizasiyɔn teliya ani a vulkanizasiyɔn hakɛ ka bon ka tɛmɛ CR2322 kan.
Mooney ka sɔgɔsɔgɔninjɛ cayara kosɛbɛ ni CR hakɛ cayara. CR2322 bɛ caya ka tɛmɛ CR3222 kan ni CR hakɛ cayara, nka CR3222 bɛ bonya ni CR hakɛ kelen kɛra.
2.2 CR suguya ni a tata hakɛ danfaralenw nɔ min bɛ V-belt compression rubber farikolo ni a kɛcogo la
Ni CR2322 tata hakɛ cayara, fɛn bɛɛ lajɛlen jiginni fanga bɛrɛbɛrɛ tɛ kɛ kosɛbɛ, janya bɛ dɔgɔya kari waati la, sɛgɛn degun ni gɛlɛya bɛ bonya 100%. Wa ni 100 °C ye ni kɔrɔya waati janya ye, sɔgɔli fanga, ɲɛjibɔ janya bɛ dɔgɔya ani ni CR2322 hakɛ cayara, sɔgɔli fanga, tigɛ janya bɛ dɔgɔya ka dɔgɔn ni kɔrɔya waati janya ye 100% janya ye tuma bɛɛ, a gɛlɛya bɛ bonya, ani CR2322 hakɛ danfaralenw, 100% janya basigilen, gɛlɛya bɛ bonya ni danfara fitinin ye, nka u ka dɔgɔn ka tɛmɛ furakisɛ kan min tɛ CR2322 ye.
Ni CR3222 hakɛ cayara ni a ma kɔrɔbaya, a sɔgɔli fanga ma Changé kosɛbɛ, a tension janya dɔgɔyara, 100% tension degun basigilen bɛ dɔgɔya fɔlɔ ka sɔrɔ ka bonya, wa a gɛlɛya ma Changé kosɛbɛ. Wa ni 100 °C sigida la ni kɔrɔya waati janya ye, sɔgɔli fanga, tigɛli janya bɛ dɔgɔya ani CR3222 sɔgɔli fanga hakɛ danfaralenw, tigɛli janya dɔgɔyara ni hakɛ fitinin ye, nka u ka dɔgɔn ka tɛmɛ furakisɛ kan min tɛ CR3222 ye ni 100% jɔlen kɔrɔya waati janyalen don, gɛlɛya bɛ bonya, ani CR3222 hakɛ danfaralenw 100% sɔgɔli jɔlen na, gɛlɛya bonya tɛ danfaraba don. Kɔrɔya waati danfaralenw kɔnɔ CR hakɛ kelen na 100 °C la, CR3222 ka sɛgɛn fanga yeli hakɛ bɛ dɔgɔya ka tɛmɛ CR2322 ta kan ni kɔrɔya waati janyalen don CR3222 ni CR2322 ka sɔgɔsɔgɔninjɛ janya, 100% janya, ani Shore A gɛlɛya yeli hakɛ tɛ danfaraba don ni CR2322 ta ye.
Sisan sulfure siratigɛ la, CR2322 ka flexural property ka fisa kosɛbɛ ni CR3222 ta ye 80 °C la, wa ni CR2322 hakɛ bɛ caya, flexural property ɲuman bɛ sɔrɔ ni CR2322 hakɛ ye tilayɔrɔ 20 ye, ani flexural property bɛ tiɲɛ ni CR3222 hakɛ bɛ caya.
2.3 Mullins nɔ min bɛ CR suguya ni a tata hakɛ danfaralenw na V-belt Compression Adhesives kan
Since the compression rubber is subjected to repetitive compression stress during normal use, and the Mullins effect under compression characterizes the stress softening of vulcanized rubber under repetitive compression, the compression rubber needs to have good stiffness under cyclic compression stress, and the stress softening should be as small as possible, so the Mullins effect under compression is used to characterize the state of compression rubber ka degun nɔgɔyali. V-belt gansanw ka funteni hakɛ bɛ se 80 °C ɲɔgɔn ma, o la walasa ka compression adhesive baaracogo nɔgɔman ladege, Mullins effect min bɛ 80 °C la, o sɛgɛsɛgɛra walasa ka jamana baaracogo lakika jira.
Ni CR2322 hakɛ cayara, degun fanga min ka bon kosɛbɛ, o bɛ bonya ka kɔn 100°C×24h kɔrɔya ɲɛ ani a kɔfɛ. Ni CR2322 hakɛ min bɛ kɛ, o ye kelen ye, degun fanga min ka bon kosɛbɛ, o bɛ bonya kosɛbɛ 100 °C × 24 h kɔrɔya kɔfɛ. Ikomi danfara fitinin min bɛ degun fanga fɔlɔ ni sabanan cɛ, o b’a jira ko Mulins nɔ bɛ barika dɔgɔya, a jɛlen don ko Mulins nɔ bɛ barika dɔgɔya ni CR2322 hakɛ caya ye, wa Mulins nɔ bɛ barika dɔgɔya hali bi ni CR2322 hakɛ cayara kɔrɔya kɔfɛ 100 °C × 24 h la. Nka, n’i y’a suma ni min ye sani mɔgɔ ka kɔrɔbaya, degun fanga hakɛ min ka bon kosɛbɛ, o bɛ bonya ka kɔn kɔrɔya ɲɛ ani kɔrɔya kɔfɛ. Nka ni i ye a suma ni min kɛra sani mɔgɔ ka kɔrɔ, Mulins nɔ hakɛ cayara 100 °C × 24 h kɔrɔya kɔfɛ, ani Mulins nɔ hakɛ cayara ni CR2322 tata hakɛ cayara.
CR3222 ni CR2322 cogoya bɛ tali kɛ ɲɔgɔn na Mullins nɔfɛko siratigɛ la. Ni an ye CR3222 ni CR2322 suma ɲɔgɔn na waatijan kɔnɔ, o b’a jira ko fanga camanba siratigɛ la, CR3222 ka bon kosɛbɛ ka tɛmɛ CR2322 kan CR hakɛ kelen na, wa o cogo kelen de bɛ kɛ kɔrɔya kɔfɛ 100 °C × 24 h la. Mulins nɔfɛko siratigɛ la, danfara min bɛ Mulins nɔfɛta la CR3222 ni CR2322 cɛ CR hakɛ kelen na sani a ka kɔrɔya 100 °C × 24 h la, o tɛ belebele ye, nka danfara min bɛ Mullins nɔ na CR2322 ni CR322 cɛ 100 °C × 24 h la, o man bon. Nka, kɔrɔya kɔfɛ 100 °C × 24 h la, CR3222 ka Mullins nɔ bɛ dɔgɔya ka tɛmɛ CR2322 ta kan CR hakɛ kelen na.
2.4 CR suguya ni hakɛ danfaralenw nɔ min bɛ V-belt compression rubber ka funteni sɔrɔli fangama na
Tɔnɔ hakɛ (tanδ), n’o ye fasa danfara yɔrɔ ye min bɛ fɛn viskoelasitiki dɔ ka sɛgɛn ni a degun sɛrɛkili cɛ fanga foro ɲɔgɔn falen-falen wale kɔrɔ, o fana bɛ bɛn bɔnɛ hakɛ ni fɛn in fanga marali modulu hakɛ ma, wa a ye taamasiyɛn nafama ye walasa ka lastikuw ka funteni sɔrɔli fangama suman. O de kama, CR suguya ni hakɛ danfaralenw nɔ minnu bɛ V-belt compression rubber tanδ kan, olu sɛgɛsɛgɛra.
Ni sɛgɛsɛgɛli funteni ka bon, ni lastikuw vulkanizelen ka tanδ bɛ dɔgɔya, ani ni lastikuw vulkanizelen tanδ bɛ bonya ni CR kɛli ye, o bɛ tali kɛ a la ko CR bɛ ni Cl kɛrɛfɛ kulu ye a ka molekiyɔmu jɔcogo la.
O bɛ tali kɛ Cl fan kulu la CR ka molekiyɔmu jɔcogo la. Lastikuw vulkanizelen ka tanδ bɛ dɔgɔya ni CR2322 hakɛ cayara, nka danfara tɛ ye ni funteni dɔgɔyara ni 100°C ye. Ka fara o kan, vulcanized rubber tanδ bɛ dɔgɔya ni CR3222 hakɛ cayara, nka danfara tɛ ye ni 100°C dɔgɔyara. Ka fara o kan, vulcanized rubber tanδ ka dɔgɔn ni CR3222 yɔrɔ 20 ye. Ni an y’a suma ni janya ye, CR3222 ka tanδ ka dɔgɔ ni CR2322 ta ye funteni kelen na ani CR hakɛ kelen na, o bɛ se ka kɛ sababu ye ka danfara don furakɛli lastikuw ka tanδ la ka da danfara kan molekiyɔmu jɔcogo ni vulkanizasiyɔn sitɛmu wajibiyalen na fan kelen fɛ, ani ka da danfara kan furakɛli lastikuw tanδ la k’a sababu kɛ danfara ye cross-linking density kan fan dɔ fɛ.
3 Kuncɛli
(1) Ni CR2322 tali cayara, t 10 ni t 90 surunyara ka sɔrɔ ka janya, wa M HM L ma Changé kosɛbɛ. Ni CR3222 cayara, t 10 ni t 90 surunyara ani M HM L cayara dɔɔnin dɔɔnin. Mooney ka sɔgɔsɔgɔninjɛ bɛ bonya kosɛbɛ ni CR hakɛ cayara, wa CR2322 ka bon ni CR3222 ye amplitude bonya siratigɛ la, nka CR3222 nafa bɛ bonya ni CR hakɛ kelen kɛra.
(2) Ni dɔ farala CR2322 tali kan, a bɛɛ lajɛlen ka fɛnɲɛnamafagalan tɛ Changé kosɛbɛ, a fɛnɲɛnamafagalan fanga bɛ dɔgɔya, 100% janya ni a gɛlɛya bɛ bonya. Ni CR3222 cayara, sɛgɛn fanga tɛ Changé kosɛbɛ, janya bɛ dɔgɔya ɲɛjibɔ waati, janya degun 100% bɛ dɔgɔya ka sɔrɔ ka bonya, wa a gɛlɛya tɛ Changé kosɛbɛ. CR fila bɛɛ farikolo ni u ka masinko marali hakɛ cayara kɔrɔya kɔfɛ 100°C × 24 h la. Sisan vulcanization system fana Sɔrɔla ko farikolo ni masin nafaw marali hakɛ ka bon. Sisan vulkanizasiyɔn siratigɛ la, CR2322 ka flexural resistance ka fisa kosɛbɛ ni CR3222 ta ye 80°C la.
(3) Ni CR hakɛ bɛ caya, Mullins nɔ bɛ dɔgɔya ani fanga min ka bon kosɛbɛ, o bɛ bonya. Fanga hakɛ caya siratigɛ la, a jɛlen don ko CR3222 ka bon ni CR2322 ye CR hakɛ kelen na, wa a fana bɛ kɛ kelen ye kɔrɔya kɔfɛ 100 °C × 24 h la. Mulins nɔ ta fan fɛ, sani mɔgɔ ka kɔrɔya 100 °C × 24 h la, danfaraba tɛ CR3222 ni CR2322 cɛ Mullins nɔ ta fan fɛ CR hakɛ kelen na, nka kɔrɔya kɔfɛ 100 °C × 24 h la, CR3222 ni CR2322 ka kɔrɔtacogo ka fisa kosɛbɛ ka tɛmɛ CR2322 kan CR kelen na a tata hakɛ. Nka, kɔrɔya kɔfɛ 100 °C × 24 h la, CR3222 ka Mullins nɔ bɛ dɔgɔya ka tɛmɛ CR2322 ta kan CR hakɛ kelen na.
(4) Lastikuw vulkanizelen ka tanδ bɛ dɔgɔya ni CR2322 baara caya ye, nka danfara tɛ ye ni a ma se 100 °C ma. Ka fara o kan, ni CR3222 hakɛ bɛ caya, lastikuw vulkanizelen tanδ bɛ dɔgɔya ni CR3222 hakɛ ye tilayɔrɔ 20 ye. CR3222 tanδ ka dɔgɔn ni CR2322 ta ye sɛgɛsɛgɛli funteni kelen na ani CR hakɛ kelen na.