Views: 0 Author: Site Editor Ɣeyiɣi si Wotae: 2023-08-13 Dzɔtsoƒe: Teƒe
Compression rubber na V-belts dzrowo le duta dukɔwo me ƒe akpa gãtɔ nye SBR/dzɔdzɔme rabber ŋutilã kple chloroprene rubber aɖewo. Transmission belt nye ŋusẽ zazã le rababa nuwɔna, ele be mɔfiame la nabu ŋusẽ cranking dɔwɔwɔ, dzoxɔxɔ dzidzi, nutsyɔnu rababa hã ele be woabu abrasion tsitretsitsi, rababa ƒe agbɔsɔsɔme mele be wòaɖiɖi akpa o. Wozãa ʋukuku ƒe alidziblanu siwo ƒe nyonyome deŋgɔ abe V-belts kpuiwo, agbledelawo ƒe V-belts, V-belts siwo ƒe nugbɔwo wotso, multiribbed belts kple synchronous belts geɖe le chloroprene rababa me. chloroprene rababa ƒe ŋusẽ sẽ, dzoxɔxɔ te ŋu nɔa te ɖe enu, te ŋu nɔa te ɖe tsitsi nu, te ŋu nɔa te ɖe ozone nu, te ŋu nɔa te ɖe abrasion nu, ɖeɖi tea eŋu nyuie le ƒoƒo me, eye wòléna ɖe nu bubuwo ŋu nyuie. Dzoxɔxɔ ƒe didime si sɔ la nye -30 ~ 100°C zi geɖe. Dutatɔwo ƒe dɔlékuiwo kaka ƒe alidziblanu akpa gãtɔ zãa chloroprene rababa si wozãna le mɔ gbadza nu si ƒe kristalo mede o. Nusiwo gbɔna nye neoprene ƒe hatsotso eve siwo wozã le numekuku sia me ƒe dɔwɔwɔ ƒe dzesiwo
CR232: Atike sia nye chloroprene polymer si me diisopropyl dithiocarbonate nye ɖoɖowɔla. Crystallization ƒe duƒuƒu le titina, density nye 1.23, beige lumps, meƒoa ɖi o. Dzoxɔxɔ ƒe tsitretsitsi nyuie le esi eye wòli ke le dzoxɔxɔ gã me. Woate ŋu azãe na rababa ƒomevi ɖesiaɖe si ƒe amadede le keklẽm, abe nutrenuwo, ke ƒe nutsyɔnu, agbalẽxatsaxatsa, nutsyɔnu, hose ƒe gotagome kotoku kple rababa ƒe akpa vovovo bubuwo ene. Atike sia sɔ kple DuPont ƒe W-ƒomevi kple Nidec ƒe M-40-ƒomevi chloroprene rababa.
CR322: Atike sia nye chloroprene polymer si me sulfur kple diisopropyl dithiocarbonate le abe nusi wotsɔ tsakae kple esi trɔa asi le eŋu ene. Crystallization ƒe duƒuƒu le titina, density 1.23, beige alo brown lumps, meƒoa ɖi o. Aɖatsi ƒe ŋusẽ gã, dɔwɔwɔ ƒe dɔwɔwɔ nyo wu sulfur-regulated rubber. Woateŋu azãe le kaƒomɔ̃wo, mɔ̃ siwo tsɔa nu kple rababa bubuwo wɔwɔ me. Adzɔnu sia sɔ kple DuPont GW ƒomevi ƒe rababa.
2.1 Ŋusẽkpɔɖeamedzi si CR ƒe hatsotso vovovowo kple eƒe agbɔsɔsɔme kpɔna ɖe vulcanization ƒe dɔwɔwɔ kple Mooney viscosity dzi le V-belt compression rubber me.
Ne CR2322 ƒe agbɔsɔsɔme dzi ɖe edzi la, t 10, t 90 gbã kpuie eye emegbe wòdidi, esia le alea elabena CR2322 nye non-sulphur-conditioned, ZnO, MgO abe CR2322 sulfurizing agent ƒe agbɔsɔsɔme si woɖo ɖi ene, CR2322 ƒe agbɔsɔsɔme sɔ kple relative sulfurizing agent si le CR ɖesiaɖe me la le sue wu, eyata zi nenemae lolo wu agbɔsɔsɔme si nye CR2322 t 10, t 90 didi wu. Eye M HM L metrɔna boo o. Tsɔ kpe ɖe eŋu la, ne CR3222 ƒe agbɔsɔsɔ le dzidzim ɖe edzi la, t 10 kple t 90 nɔa kpuie wu. Esia tso nyateƒe si wònye be CR3222 nye ƒomevi si wotsaka eye wotrɔ asi le eŋu, ZnO, MgO kple S wɔa dɔ ɖekae abe vulcanizing agents ene, eye esi CR ŋutɔ ƒe coking ɣeyiɣi le kpuie eye wòwɔa kabakaba wu NR/BR ta la, vulcanization ƒe duƒuƒu va nɔa kabakaba ne CR3222 ƒe agbɔsɔsɔme dzi ɖe edzi, eye M HM L dzina ɖe edzi vivivi. Mlɔeba la, le vulcanization ɖoɖo si li fifia nu la, CR3222 ƒe dzobibi ƒe ɣeyiɣi le kpuie, vulcanization ƒe tsɔtsɔme kabakaba eye vulcanization ƒe agbɔsɔsɔme sɔ gbɔ wu CR2322.
Mooney ƒe ʋeʋẽ dzi ɖe edzi ŋutɔ esi CR ƒe agbɔsɔsɔme dzi ɖe edzi. CR2322 dzina ɖe edzi wu CR3222 ne CR ƒe agbɔsɔsɔme dzi ɖe edzi, gake CR3222 lolona wu ne wozã CR ƒe agbɔsɔsɔ ma ke.
2.2 Ŋusẽ si CR ƒe hatsotso vovovowo kple eƒe agbɔsɔsɔme kpɔna ɖe V-belt compression rubber ƒe ŋutilã kple mɔ̃ɖaŋununya ƒe nɔnɔmewo dzi
Ne CR2322 ƒe agbɔsɔsɔme dzi ɖe edzi la, tɔtrɔ bliboa le tensile strength me meɖe dzesi o, elongation le break dzi ɖena kpɔtɔna, 100% tensile stress kple hardness dzina ɖe edzi. Eye le 100 °C kple tsitsi ƒe ɣeyiɣi didi la, tensile strength, tearing elongation dzi ɖe kpɔtɔ eye zi alesi CR2322 ƒe agbɔsɔsɔme sɔ gbɔe la, tensile strength, tearing elongation dzi ɖe kpɔtɔ vie; kple tsitsi ƒe ɣeyiɣi didi si nye 100% ƒe didime ɣesiaɣi, sesẽme dzi ɖe edzi, eye CR2322 ƒe agbɔsɔsɔme vovovowo, 100% ƒe didime ɣesiaɣi, sesẽme dzi ɖe edzi to vovototo sue aɖe me, gake wole sue wu mɔli si me CR2322 mele o.
Esi CR3222 ƒe agbɔsɔsɔme dzi ɖe edzi ne metsi o la, tensile strength metrɔ boo o, tensile elongation dzi ɖe kpɔtɔ, 100% constant tensile stress dzi ɖe kpɔtɔ gbã eye emegbe wòdzi ɖe edzi, eye sesẽme metrɔ boo o. Eye le 100 °C nɔnɔme me kple tsitsi ƒe ɣeyiɣi kekeɖenudɔ, tensile ŋusẽ, tearing elongation dzi ɖe kpɔtɔ eye vovovo dosage CR3222 tensile ŋusẽ, tearing elongation dzi ɖe kpɔtɔ vie, gake wole sue wu formula si me CR3222 mele o; kple tsitsi ƒe ɣeyiɣi didi si le 100% fixed tensile la, sesẽme dzina ɖe edzi, eye CR3222 ƒe agbɔsɔsɔme vovovowo le 100% fixed tensile la, sesẽme ƒe dzidziɖedzi meto vovo boo o. Le tsitsi ƒe ɣeyiɣi vovovo siwo me CR ƒe agbɔsɔsɔ ɖeka le le 100 °C me la, CR3222 ƒe tensile strength ƒe tɔtrɔ ƒe agbɔsɔsɔme le sue wu CR2322 tɔ ne tsitsi ƒe ɣeyiɣi didi; tɔtrɔ ƒe agbɔsɔsɔme si le vuvu ƒe didime, 100% ƒe didime, kple Shore A ƒe sesẽme si le CR3222 kple CR2322 me meto vovo boo tso CR2322 tɔ gbɔ o.
Le sulfide ƒe ɖoɖo si li fifia nu la, CR2322 ƒe flexural nɔnɔme nyo wu CR3222 tɔ le 80 °C me sã, eye ne CR2322 ƒe agbɔsɔsɔ le dzidzim ɖe edzi la, flexural property nyuitɔ kekeake nɔa anyi ne CR2322 ƒe agbɔsɔsɔme nye akpa 20, eye flexural property la gblẽna ne CR3222 ƒe agbɔsɔsɔ le dzidzim ɖe edzi.
2.3 Mullins ƒe Ŋusẽkpɔɖeamedzi si CR ƒe Dzeside vovovowo kple Agbɔsɔsɔme Vovovowo kpɔna ɖe V-belt Compression Adhesives dzi
Esi wònye be wotsɔa nutete ƒe rababa la dea nutete ƒe nuteɖeamedzi enuenu me le ezazã si sɔ me, eye Mullins ƒe ŋusẽkpɔɖeamedzi le nutete te ɖea dzesi le nuteɖeamedzi ƒe fafa si le rababa si wotsɔ vulcanized wɔe me le nutete enuenu te ta la, ele be nutete ƒe rababa la nasẽ nyuie le nutete ƒe nuteɖeamedzi si le tsatsam te, eye ele be nutete ƒe fafa nanɔ sue alesi wòanya wɔe, eyata wozãa Mullins ƒe ŋusẽkpɔɖeamedzi le nutete te tsɔ dea dzesi nɔnɔme si me compression rubber ƒe nuteɖeamedzi ƒe fafa. V-belt dzrowo ƒe dzoxɔxɔ si sɔ la anɔ abe 80 °C ene, eyata be woate ŋu awɔ alesi wozãa nutete ƒe aŋenu la le mɔ nyuitɔ nu la, wodo Mullins ƒe ŋusẽkpɔɖeamedzi si le 80 °C me kpɔ be wòaɖe nɔnɔmea zazã ŋutɔŋutɔ afia.
Ne CR2322 ƒe agbɔsɔsɔ dzi ɖe edzi la, nutete ƒe ŋusẽ si sɔ gbɔ wu dzina ɖe edzi do ŋgɔ na tsitsi 100°C×24h kple emegbe. Ne CR2322 ƒe xexlẽme si wozã sɔ la, nutete ƒe ŋusẽ si sɔ gbɔ wu dzina ɖe edzi ŋutɔ le tsitsi 100 °C × 24 h megbe. Esi wònye be vovototo sue si le nuteteŋusẽ gbãtɔ kple etɔ̃lia dome ɖee fia be Mullins ƒe ŋusẽkpɔɖeamedzia gbɔdzɔ wu ta la, edze ƒã be Mullins ƒe ŋusẽkpɔɖeamedzia gbɔdzɔna ne CR2322 ƒe agbɔsɔsɔ dzi ɖe edzi, eye Mullins ƒe ŋusẽkpɔɖeamedzia gakpɔtɔ gbɔdzɔna ne CR2322 ƒe agbɔsɔsɔ dzi ɖe edzi le tsitsi le 100 °C × 24 h megbe. Gake ne wotsɔe sɔ kple esi do ŋgɔ na tsitsi la, nutete ƒe ŋusẽ si sɔ gbɔ wu dzina ɖe edzi do ŋgɔ na tsitsi kple emegbe. Gake ne wotsɔe sɔ kple esi do ŋgɔ na tsitsi la, Mullins ƒe ŋusẽkpɔɖeamedzi ƒe agbɔsɔsɔme dzi ɖe edzi le tsitsi 100 °C × 24 h megbe, eye Mullins ƒe ŋusẽkpɔɖeamedzi ƒe agbɔsɔsɔme dzi ɖe kpɔtɔ ne CR2322 ƒe agbɔsɔsɔme dzi ɖe edzi.
CR3222 ƒe nɔnɔme sɔ kple CR2322 le Mullins ƒe ŋusẽkpɔɖeamedzi gome. CR3222 kple CR2322 ƒe tsɔtsɔ sɔ kple wo nɔewo le ɣeyiɣi didi me ɖee fia be le ŋusẽ si sɔ gbɔ wu gome la, CR3222 lolo ŋutɔ wu CR2322 le CR ƒe agbɔsɔsɔme ma ke me, eye nenema ke wòle le tsitsi le 100 °C × 24 h megbe. Le Mullins ƒe ŋusẽkpɔɖeamedzi gome la, vovototo si le Mullins ƒe ŋusẽkpɔɖeamedzi me le CR3222 kple CR2322 dome le CR ƒe agbɔsɔsɔme ɖeka me hafi woatsi le 100 °C × 24 h me lolo o, gake vovototo si le Mullins ƒe ŋusẽkpɔɖeamedzi me le CR2322 kple CR322 dome le 100 °C × 24 h dome la melolo o. Gake le tsitsi le 100 °C × 24 h megbe la, CR3222 ƒe Mullins ƒe ŋusẽkpɔɖeamedzi gbɔdzɔna wu CR2322 tɔ le CR ƒe agbɔsɔsɔme ma ke me.
2.4 Ŋusẽ si CR ƒe hatsotso vovovowo kple eƒe agbɔsɔsɔme kpɔna ɖe dzoxɔxɔ si trɔna si le V-belt compression rubber me dzi
Nusiwo bu (tanδ), si nye tangent si le phase ƒe vovototo ƒe dzogoe si le viscoelastic nusi ƒe tete kple nuteɖeamedzi ƒe tsatsam dome le ŋusẽ ƒe agble si trɔna ƒe dɔwɔwɔ te, hã sɔ kple nusiwo bu ƒe modulus kple nusi ƒe ŋusẽdzraɖoƒe ƒe modulus ƒe sɔsɔme, eye wònye dzesi vevi aɖe na dzoxɔxɔ ƒe dzidziɖedzi si le ŋusẽ kpɔm le rababa ƒe nuwɔna me dzidzedze. Eyata wowɔ numekuku le ŋusẽ si CR ƒe hatsotso vovovowo kple agbɔsɔsɔ vovovowo kpɔna ɖe V-belt compression rubber ƒe tanδ dzi ŋu.
Zi alesi dodokpɔa ƒe dzoxɔxɔ loloe la, zi nenemae rababa si wotsɔ vulcanized wɔe ƒe tanδ bɔbɔna, eye zi nenemae tanδ si le rababa si wotsɔ vulcanized wɔe ƒe tanδ dzina ɖe edzi ne wozã CR la, esia do ƒome kple nyateƒe si wònye be Cl ƒe axadzi ƒuƒoƒo le CR le eƒe molecule ƒe wɔwɔme me.
Esia do ƒome kple Cl axadzi ƒuƒoƒo si le CR ƒe molecule ƒe wɔwɔme me. Rababa si wotsɔ vulcanized wɔe ƒe tanδ dzi ɖena kpɔtɔna ne CR2322 ƒe agbɔsɔsɔ dzi ɖe edzi, gake vovototoa medzena ne dzoxɔxɔa ɖiɖi wu 100°C o. Tsɔ kpe ɖe eŋu la, rababa si wotsɔ vulcanized wɔe ƒe tanδ dzi ɖena kpɔtɔna ne CR3222 ƒe agbɔsɔsɔ dzi ɖe edzi, gake vovototoa medzena le dzoxɔxɔ si mede 100°C o me o. Gawu la, tanδ si le rababa si wotsɔ vulcanized wɔe lae nye suetɔ kekeake le CR3222 ƒe akpa 20 me. Le didime tsɔtsɔ sɔ kple wo nɔewo me la, CR3222 ƒe tanδ bɔbɔ wu CR2322 tɔ le dzoxɔxɔ ɖeka kple CR ƒe agbɔsɔsɔ ɖeka me, si ate ŋu atso vovototo si le tanδ me le curing rubber la me le vovototo si le molecule ƒe wɔwɔme kple vulcanization system si hiã me le akpa ɖeka, kple le vovototo si le tanδ me le curing rubber la me le vovototo si le cross-linking density le edzi ta akpa kemɛ.
3 Nyataƒoƒo
(1) Esi CR2322 zazã dzi ɖe edzi la, woɖe t 10 kple t 90 dzi kpɔtɔ eye emegbe wodidi, eye M HM L metrɔ boo o. Esi CR3222 dzi ɖe edzi la, woɖe t 10 kple t 90 dzi kpɔtɔ eye M HM L dzi ɖe edzi vivivi. Mooney ƒe ʋeʋẽ dzina ɖe edzi ŋutɔ ne CR ƒe agbɔsɔsɔme dzi ɖe edzi, eye CR2322 lolo wu CR3222 le amplitude ƒe dzidziɖedzi gome, gake CR3222 ƒe asixɔxɔ lolona wu ne wozã CR ƒe agbɔsɔsɔ ma ke.
(2) Ne CR2322 zazã dzi ɖe edzi la, tensile strength bliboa metrɔna boo o, tensile strength dzi ɖena kpɔtɔna, 100% elongation kple hardness dzina ɖe edzi. Ne CR3222 dzi ɖe edzi la, tensile strength metrɔna boo o, elongation le aɖatsi me dzi ɖena kpɔtɔna, 100% elongation stress dzi ɖena kpɔtɔna eye emegbe wòdzina ɖe edzi, eye sesẽme metrɔna boo o. CR eveawo ƒe dzɔdzɔme kple mɔ̃ɖaŋununya ƒe nɔnɔmewo ƒe léle ɖe asi dzi ɖe edzi le tsitsi le 100°C × 24 h megbe. Wokpɔe hã be vulcanization ɖoɖo si li fifia la léa ŋutilã kple mɔ̃ɖaŋununya ƒe nɔnɔmewo ɖe te ŋutɔ. Le vulcanization ɖoɖo si li fifia te la, CR2322 ƒe flexural resistance nyo wu CR3222 tɔ le dzoxɔxɔ 80°C me sã.
(3) Ne CR ƒe agbɔsɔsɔ dzi ɖe edzi la, Mullins ƒe ŋusẽkpɔɖeamedzi dzi ɖena kpɔtɔna eye ŋusẽ si sɔ gbɔ wu dzina ɖe edzi. Le ŋusẽ si sɔ gbɔ wu gome la, edze ƒã be CR3222 lolo wu CR2322 le CR ƒe agbɔsɔsɔme ma ke me, eye nenema ke hã le tsitsi le 100 °C × 24 h megbe. Le Mullins ƒe ŋusẽkpɔɖeamedzi gome la, hafi woatsi le 100 °C × 24 h me la, vovototo boo aɖeke mele CR3222 kple CR2322 dome le Mullins ƒe ŋusẽkpɔɖeamedzi le CR ƒe agbɔsɔsɔme ɖeka me o, gake le tsitsi le 100 °C × 24 h megbe la, CR3222 kple CR2322 ƒe flexural nɔnɔmewo nyo wu CR2322 le CR ɖeka me agbɔsɔsɔme si wozãna. Gake le tsitsi le 100 °C × 24 h megbe la, CR3222 ƒe Mullins ƒe ŋusẽkpɔɖeamedzi gbɔdzɔna wu CR2322 tɔ le CR ƒe agbɔsɔsɔme ma ke me.
(4) Rababa si wotsɔ vulcanized wɔe ƒe tanδ dzi ɖena kpɔtɔna ne wozã CR2322 geɖe wu, gake vovototoa medzena gaglãa ne mede 100 °C o. Tsɔ kpe ɖe eŋu la, ne CR3222 ƒe agbɔsɔsɔ le dzidzim ɖe edzi la, tanδ si le rababa si wotsɔ vulcanized wɔe me nyea suetɔ kekeake ne CR3222 ƒe agbɔsɔsɔme nye akpa 20. CR3222 ƒe tanδ le ʋɛ wu CR2322 tɔ le dodokpɔ ƒe dzoxɔxɔ ɖeka kple CR ƒe agbɔsɔsɔme ɖeka me.