Ukubuka: 0 Umbhali: Isikhathi Sokushicilela Isihleli Sesayithi: 2023-08-15 Umsuka: Isayithi
Njengenye yezinto zokuqala ezasetshenziswa embonini yenjoloba, indima ye-zinc oxide ibilokhu ishintsha ngokuthuthukiswa kobuchwepheshe benjoloba.
Kusukela ku-ejenti yokuqala yombala, i-ejenti eqinisayo ukuya ohlelweni lwe-vulcanization ingafinyeza isikhathi se-vulcanization ye-ejenti esebenzayo, irabha ye-chloroprene kanye nerabha ye-carboxy ku-ejenti ephazamisayo, izimo eziguquguqukayo zemikhiqizo yenjoloba esetshenziswa ku-thermal conductivity ye-filler, njll., okuthi njenge-vulcanization system, i-zinc oxide esebenza kakhulu isasebenza. I-Magnesium oxide ingasetshenziswa futhi njenge-ejenti esebenzayo ekuvuthweni kwenjoloba, kodwa ngenxa yomsebenzi ophansi kanye nezakhiwo ezibonakalayo zezinto zenjoloba zimpofu, ngakho-ke i-magnesium oxide isetshenziswa kakhulu njenge-agent e-vulcanizing kanye ne-stabilizer yokushisa ku-rubber equkethe i-halogen.
I-peroxide vulcanization i-peroxide kanye nerabha enqubweni ye-vulcanization kwenzeka ukusabela kwamahhala kwe-radical ukuze kwakhiwe ibhondi ephakeme ye-cc yamandla.
Uma kuqhathaniswa ne-sulphur yellow vulcanization, inezinzuzo zokumelana nokushisa okuhle, ukucindezela okuhle kakhulu kokusebenza kokuguqulwa okuhlala njalo, akulula ukufafaza isithwathwa, nokuxhumana okulula, njll. Eminyakeni yamuva, isetshenziswe kabanzi emikhiqizweni yenjoloba ngaphansi kwezimo zokushisa eziphakeme. Kusukela ku-cross-linking mechanism, i-peroxide vulcanization system ayikwazi ukucushwa ngama-oxide ensimbi, kodwa enqubweni yangempela yokukhiqiza, abantu basavame ukwengeza izingxenye ezi-5 zama-oxide ensimbi kufomula, kanye nokusetshenziswa kwayo okuqondile komphumela wemibono ehlukene. Ucwaningo lubonisa ukuthi i-nano zinc oxide, i-magnesium oxide, i-calcium oxide ne-unsaturated acid ingasetshenziswa njenge-ejenti entsha ye-co-crosslinking ku-peroxide vulcanized hydrogenated nitrile butadiene rubber (HNBR), enganciphisa isikhathi se-vulcanization futhi ithuthukise ukuminyana kwe-crosslink kanye nezakhiwo zomzimba, kodwa umphumela wokumelana nokushisa kwerabha awukhulunywa.
1. Umphumela we-zinc oxide noma i-magnesium oxide ezintweni zenjoloba
Uma kuqhathaniswa nesampula elingenalutho, ukungezwa kwe-zinc oxide noma i-magnesium oxide rubber M kuye kwanda, futhi i-zinc oxide rubber ML iphakeme, lokhu kungenxa yokuthi i-zinc oxide inendawo engaphezulu kanye nomphumela oqinile wokuhlangana, ku-matrix yenjoloba akulula ukuyihlakaza, kulula ukuhlanganisa, ukuhlanganisa, okubangela uketshezi lwenjoloba lwe-ML lukhuphuke, lukhuphuke. Ukwengezwa kwama-oxide ensimbi nakho kwandisa i-MH-ML yenhlanganisela, okubonisa ukuthi ama-oxide ensimbi angakhuthaza ukuxhumanisa, athuthukise izinga le-vulcanization, kodwa futhi afinyeze i-T10 kodwa abe nomthelela omncane ku-T90. Ukwengeza, i-MH-ML yezinhlanganisela ze-zinc oxide yayiphezulu kunaleyo ye-magnesium oxide compounds ngesilinganiso esifanayo, okubonisa ukuthi i-zinc oxide inomphumela omkhulu wokuvula i-vulcanization kune-magnesium oxide ohlelweni lwe-peroxide vulcanization.
Ngokukhuphuka komthamo we-zinc oxide ne-magnesium oxide, amandla okuqinile enjoloba ethintekile ayanda kuqala bese ehla, ukuthambekela okungapheli kwe-elongation okungu-100% kuyanda, kuyilapho ukunwetshwa ngesikhathi sokuphumula kanye namandla okudabula kuwumkhuba oyanciphayo, futhi esikalini esifanayo se-zinc oxide rubber impahla ehlala njalo yokwelula, le nsimbi ye-vuxual oxide iphakeme kunerubha ye-magnesium oxide iphezulu kune-elongation ye-magnesium. yethrendi ye-MH-ML, kodwa uma umthamo we-zinc oxide uyizingxenye ezingu-10 ze-100% yengcindezi ehlala njalo yokwelulwa kwenjoloba evuvukele kuwumkhuba ukwehla, okungase kubangelwe ukungahlakazwa kahle kwe-zinc oxide. Kodwa-ke, lapho umthamo we-zinc oxide wawuyizingxenye ezingu-10, ukucindezeleka okungaguquki okungu-100% kokwelulwa kwenjoloba eshisiwe kwabonisa inkambiso enciphayo, okungenzeka kubangelwe ukuhlakazeka kabi kwe-zinc oxide. Kafushane, ukungezwa kwama-oxide ensimbi kungathuthukisa ukuminyana kwenjoloba ye-HNBR ngaphansi kohlelo lwe-peroxide vulcanization, futhi izinga lokuphambana kwenjoloba equkethe i-zinc oxide liphakeme kunalelo le-magnesium oxide ngaphansi komthamo ofanayo, kepha lapho umthamo we-zinc oxide uyingxenye eyi-10 yokuncipha kokuhlakazeka okuhlala isikhathi eside, okubangela ukwehla kwengcindezi. Kusukela kuThebula 2, kungabonakala futhi ukuthi ukungezwa kwama-oxide ensimbi kungathuthukisa ubulukhuni, kodwa ngesilinganiso sawo akushintshi kakhulu, futhi umphumela wenani lokuphindaphinda awubalulekile, lapho umthamo we-zinc oxide ungenawo umthelela omkhulu ku-DIN abrasion, i-magnesium oxide vulcanized abrasion ne-adhesive abrasion ne-dosage yayo iyanda, kodwa futhi izinga eliphansi livame ukukhuphuka. I-adhesive ye-HNBR inokumelana okuhle kakhulu nokuhuzuka.
Ukuguga kwe-HNBR kungokohlobo lokuxhumanisa iketango, olubonakala ekwehleni kobude obuqinile kanye nokwanda kokuqina namandla aqinile ngemva kokuguga. Lokhu kubonisa ukuthi ukusabela kokuxhumanisa kuyaqhubeka phakathi nenqubo yokuguga, okwandisa ukuminyana kokuxhumanisa, futhi amandla okuqina awo wonke ama-rubber akhuphuka ngemva kokuguga, okubonisa ukuthi i-HNBR inezindawo ezinhle kakhulu zokushisa okuphezulu. Ngaphezu kwalokho, ukufakwa kwe-zinc oxide ne-magnesium oxide kuthuthukisa kakhulu
Ngaphezu kwalokho, ukwengezwa kwe-zinc oxide ne-magnesium oxide kungathuthukisa kakhulu izinga lokushintsha kwe-elongation eqinile ngemva kokumelana nokushisa, futhi izinga lokushintsha kwe-elongation eqinile yezinto zenjoloba liyehla ngokunyuka komthamo wezinto ezibonakalayo, okubonisa ukumelana nokushisa okuphezulu kakhulu, okungenzeka ukuthi kungenxa yokuthi ama-oxide ensimbi ngokwawo ayingxenye yento ekwazi ukugoqa kanye ne-rubber engaguquki. iphinde ivimbele ukuhlasela kweketango lamangqamuzana omoya-mpilo, futhi ithuthukise ukusebenza kokumelana nezinga lokushisa eliphezulu kwento yenjoloba. Ngesikhathi esifanayo, ukungezwa kwe-zinc oxide kunganciphisa kakhulu ukucindezelwa kwe-deformation unomphela yerabha, kodwa ngomthamo wayo awushintshi kakhulu; i-magnesium oxide ekucindezelweni kokushintsha unomphela komthelela ayibalulekile kakhulu. Ngakho-ke, ukungezwa kwenani elifanele lama-oxide ensimbi ohlelweni lwe-peroxide vulcanization kusiza ukuthuthukisa ukumelana nokushisa kwerabha.
Lapho umthamo we-zinc oxide uyizingxenye ezi-5, ijika le-TG-DTG lezinto zenjoloba ze-HNBR, njengokubola okushisayo kwezinto zenjoloba kwavela izigaba ezimbili ezisobala kakhulu, okubangelwa ikakhulukazi amaqembu amabili ahlukene we-HNBR izinga lokushisa lokubola kwamangqamuzana lihlukile. Isigaba sokuqala ngokuyinhloko i-butyl
Isigaba sokuqala sibangelwa ikakhulukazi ukuqhekeka okushisayo kwesibopho esiphindwe kabili ku-butadiene, kanti isigaba sesibili sibangelwa ukuhamba ngebhayisikili kwengxenye yeketanga le-acrylonitrile ngesikhathi senqubo yokushisa ukuze kwakhiwe inhlanganisela ye-chelate, engaqhekeka kuphela ekushiseni okuphezulu kakhulu, ngakho-ke kunezigaba ezimbili ezicacile zokushisa ezishisayo ezivele ezigabeni ezingu-4 zokubola kwe-rubber 8, futhi izinga lokushisa le-4 le-rubber livele. ℃ , okubonisa ukuzinza okuphezulu kwe-thermal.
Izinga lokushisa lokuqala lokubola okushisayo (lapho izinga lokulahlekelwa okukhulu liyi-5%) kanye nezinga lokushisa eliphezulu lokubola kwento yenjoloba linomkhuba ofanayo, futhi ukungezwa kwama-oxide ensimbi kunganciphisa izinga eliphezulu lokulahlekelwa kwenqwaba yezinto zenjoloba, lapho izinga lokushisa lokuqala lokubola elishisayo lezingxenye ezi-5 zezinto zenjoloba ye-zinc oxide likhuphuka cishe cishe ngo-15 ℃ nezingxenye zenjoloba lapho kuqhathaniswa nezingxenye ezingenalutho zenjoloba. I-zinc oxide ingathuthukisa kakhulu ukuzinza okushisayo kwento yenjoloba, kodwa lapho isilinganiso se-zinc oxide siyizingxenye ezingu-10, ukubola kokuqala okushisayo Nokho, lapho umthamo we-zinc oxide wawuyizingxenye ezingu-10, izinga lokushisa lokuqala lokubola okushisayo lehla. Lokhu kungase kubangelwe: (1) ukungahlakazwa kahle kwe-zinc oxide; (2) i-zinc oxide eningi kakhulu ohlelweni lwe-peroxide vulcanization yakhiqiza amabhondi axhumanisa ayingozi ekuzinzeni kokushisa. Isizathu esiqondile salokhu sisazophenywa ngokwengeziwe.Izinga lokushisa lokuqala lokubola kwezingxenye ezi-5 zenjoloba ye-magnesium oxide lincishisiwe uma liqhathaniswa nelezinto zenjoloba ezingenalutho, futhi izinga lokushisa elishisayo lokubola kwezinto zenjoloba lingakhuphuka kuphela lapho inani le-magnesium oxide laliyizingxenye ezingu-10. Ukusetshenziswa kokuhlaziywa kwe-TG ukuze kubonise ukumelana nokushisa kwerabha ye-silicone, imiphumela ibonisa ukuthi ukushisa komoya okuguga kwenjoloba ye-silicone kanye nezinga lokushisa elishisayo lokubola endaweni ye-oksijini yenkambiso yenguquko kuyavumelana kakhulu, kodwa kulokhu kuhlolwa kokubili akuzange kwakha ukuxhumana okuthile, kodwa kunalokho izinga eliphezulu lokulahlekelwa okukhulu kanye nenkambiso yoshintsho ekusebenzeni komoya oshisayo, okungenzeka ukuthi ukuguga kuhambisana nezinhlobo ezahlukene zokuguga. irabha kanye nendlela ehlukile yokubola okushisayo kanye nokuhlaziywa kwe-TG kwezimo (njengomkhathi wegesi). Lokhu kungase kube ngenxa yomehluko endleleni yokubola okushisayo kwezinhlobo zenjoloba ezihlukene kanye nezimo ezihlukene zokuhlaziywa kwe-TG (isb umkhathi wegesi), ngakho-ke uma ukuhlaziywa kwe-TG kusetshenziselwa ukuhlola ukumelana nokuguga komoya oshisayo wenjoloba, ukwakheka kwangempela nezimo zokuhlola kufanele kucatshangelwe ngokucophelela.
2. i-zinc oxide / magnesium oxide kanye nokusetshenziswa kwezinamathiselo ekushiseni nasemoyeni ukumelana nokuguga kanye nomphumela wokuguga unomphela wokucindezelwa
Lapho isilinganiso se-zinc oxide / magnesium oxide siyi-7/3, kuba nomphumela we-synergistic ekusebenzeni kokuguga komoya oshisayo we-adhesive, futhi i-adhesive inokumelana nokushisa okungcono kakhulu, kuyilapho ukungezwa kwe-magnesium oxide kunomphumela omubi ekucindezelweni okungapheli kokumelana nokuguga kwe-adhesive.
Isiphetho
(1) ) Ukwengezwa kwe-zinc oxide noma i-magnesium oxide ohlelweni lwe-HNBR peroxide vulcanization kungaveza umphumela wokuvula kuzinto zenjoloba futhi kuthuthukise izinga lokuphambana kwezinto zenjoloba, futhi umsebenzi we-zinc oxide ungaphezu kwalowo we-magnesium oxide, futhi izinga lokuphambana kwezinto zenjoloba libonisa ukuthambekela okukhuphukayo nokwanda komthamo we-zinc, kodwa lapho umthamo we-zinc ungaba umphumela we-zinc, ukwehla kwengcindezi engapheli ngenxa yokuhlakazeka okungekuhle, kodwa uketshezi lwento yenjoloba kuyawohloka, okuba nomthelela omncane enanini lokubuyela emuva kanye nokumelana nokuhuzuka. Ukumelana nemihuzuko kunomphumela omncane.
(2) Ukusetshenziswa okukodwa kwe-zinc oxide noma i-magnesium oxide kungathuthukisa ngokuphawulekayo ukumelana nokushisa nomoya wokuguga kwe-peroxide vulcanized HNBR compounds, kanye nokwanda kwenani lokumelana nokushisa, ukumelana nokushisa nokumelana nemihuzuko.
Inani lokumelana nokushisa liyakhula, kuyilapho ukungezwa kwe-zinc oxide kungathuthukisa ukucindezelwa okungapheli kwe-deformation ukumelana kwerabha, kuyilapho i-magnesium oxide inomthelela omncane kuyo.
(3)Ukubola okushisayo kwerabha ye-HNBR kuyizigaba ezimbili, ukungezwa kwama-oxide ensimbi kunganciphisa izinga eliphezulu lokulahlekelwa okukhulu, izingxenye ezi-5 ze-zinc oxide zingathuthukisa kakhulu ukuzinza okushisayo kwerabha.
(4) Lapho i-zinc oxide / magnesium oxide kanye nesilinganiso esingu-7/3, ukumelana nokushisa okungcono kakhulu kwenjoloba, kodwa i-magnesium oxide inomthelela omubi ekuphikisweni kwenjoloba ekucindezelweni kokusebenza kokuguquguquka unomphela.