Tel: +86 15221953351 Imel: info@herchyrubber.com
Please Choose Your Language
LABARAI
Kuna nan: Gida » Labarai » Tasirin zinc oxide da Labarai magnesium oxide akan kaddarorin peroxide vulcanized HNBR

Tasirin zinc oxide da magnesium oxide akan kaddarorin peroxide vulcanized HNBR

Ra'ayoyi: 0     Mawallafi: Lokacin Buga Editan Yanar Gizo: 2023-08-15 Asalin: Shafin

Tambaya

A matsayin ɗaya daga cikin kayan farko da aka yi amfani da su a cikin masana'antar roba, aikin zinc oxide yana canzawa tare da haɓaka fasahar roba.

Daga wakili mai canza launi na farko, wakili mai ƙarfafawa zuwa tsarin vulcanization na iya rage lokacin vulcanization na wakili mai aiki, chloroprene rubber da carboxy roba a cikin wakili na vulcanizing, yanayi mai ƙarfi na samfuran roba da aka yi amfani da su a cikin yanayin yanayin thermal na filler, da sauransu, wanda a matsayin tsarin vulcanization na wakili mai aiki, zinc oxide shine mafi inganci har yanzu. Magnesium oxide kuma za a iya amfani da a matsayin mai aiki wakili a cikin vulcanization na roba, amma saboda da ƙananan aiki da kuma jiki Properties na roba abu ba su da kyau, don haka magnesium oxide aka yafi amfani a matsayin vulcanizing wakili da zafi stabilizer a cikin halogen dauke da roba roba.

 

Peroxide vulcanization ne peroxide da kuma roba a cikin vulcanization tsari faruwa free radical ƙari dauki don samar da mafi girma bond makamashi cc bond.

Idan aka kwatanta da sulfur rawaya vulcanization, yana da abũbuwan amfãni daga mai kyau zafi juriya, m matsawa m nakasawa yi, ba sauki fesa sanyi, da kuma sauki daidaituwa, da dai sauransu A cikin 'yan shekarun nan, an yadu amfani da roba kayayyakin karkashin high zafin jiki yanayi. Daga tsarin haɗin giciye, tsarin vulcanization peroxide ba za a iya kunna shi ta hanyar ƙarfe oxides ba, amma a cikin ainihin samar da tsari, har yanzu mutane suna ƙara kusan sassan 5 na ƙarfe a cikin ma'anar, da kuma takamaiman amfani da tasirin ra'ayi daban-daban. Nazarin ya nuna cewa nano zinc oxide, magnesium oxide, calcium oxide da unsaturated acid za a iya amfani da a matsayin sabon co-crosslinking wakili a peroxide vulcanized hydrogenated nitrile butadiene roba (HNBR), wanda zai iya rage vulcanization lokaci da kuma inganta crosslink yawa da kuma jiki Properties, amma sakamako a kan zafi juriya na roba ba a ambata.

 

1. Sakamakon zinc oxide ko magnesium oxide akan kaddarorin kayan roba

Idan aka kwatanta da samfurin blank, ƙari na zinc oxide ko magnesium oxide rubber M sun karu, kuma zinc oxide rubber ML ya fi girma, wannan shi ne saboda zinc oxide yana da babban yanki mai girma da kuma tasirin tsaka-tsakin tsaka-tsakin, a cikin matrix na roba ba sauki don tarwatsawa ba, sauƙi don haɗuwa, haɓakawa, wanda ke haifar da rubber ML ya karu, rashin ruwa mara kyau. Bugu da kari na karfe oxides kuma yana ƙara MH-ML na fili, wanda ya nuna cewa karfe oxides iya inganta crosslinking, inganta mataki na vulcanization, amma kuma gajarta T10 amma da kadan tasiri a kan T90. Bugu da ƙari, MH-ML na zinc oxide mahadi ya kasance mafi girma fiye da na magnesium oxide mahadi a daidai wannan sashi, wanda ke nuna cewa zinc oxide yana da tasiri mai tasiri akan vulcanization fiye da magnesium oxide a cikin tsarin vulcanization na peroxide.

 

Tare da karuwa na zinc oxide da magnesium oxide sashi, da tensile ƙarfi na vulcanized roba farko ya karu sa'an nan kuma ragewa, da 100% m elongation danniya gaba ɗaya hali don ƙara, yayin da elongation a karya da hawaye ƙarfi ne a ragewa Trend, kuma a cikin wannan sashi na zinc oxide roba abu akai elongation danniya ne mafi girma fiye da wannan rubber oxide abu na iya zama mafi girma fiye da wannan rubber oxide. MH-ML Trend, amma lokacin da adadin zinc oxide ya kasance sassa 10 na 100% akai-akai elongation danniya na roba vulcanized ne ragewa Trend, wanda za a iya lalacewa ta hanyar matalauta watsawa na zinc oxide. Duk da haka, lokacin da adadin zinc oxide ya kasance sassa 10, damuwa na 100% akai-akai na haɓakar ƙwayar roba ya nuna raguwar yanayin, wanda zai iya haifar da rashin talauci na zinc oxide. A taƙaice, Bugu da kari na karfe oxides iya inganta crosslinking yawa na HNBR roba karkashin peroxide vulcanization tsarin, da kuma mataki na crosslinking na zinc oxide-dauke da roba ne mafi girma fiye da na magnesium oxide a karkashin wannan sashi, amma a lokacin da sashi na zinc oxide ne 10 rabo daga matalauta tarwatsawa na m danniya, wanda ke haifar da m. Daga Table 2, ana iya ganin cewa ƙari na ƙarfe oxides na iya inganta taurin, amma tare da adadinsa ba ya canzawa da yawa, kuma sakamakon da aka yi a kan darajar rebound ba shi da mahimmanci, wanda ƙwayar zinc oxide ba ta da tasiri mai mahimmanci akan DIN abrasion, magnesium oxide vulcanized adhesive abrasion tare da adadinsa yana ƙaruwa kuma yana nuna ƙarar matakin gabaɗaya, amma har yanzu yana nuna ƙarar matakin gabaɗaya. HNBR m yana da kyakkyawan juriya abrasion.

 

A tsufa na HNBR nasa ne da sarkar giciye-linking irin, wanda aka bayyana a cikin rage tensile elongation da karuwa da taurin da tensile ƙarfi bayan tsufa. Wannan yana nuna cewa haɗin gwiwar haɗin gwiwar yana ci gaba a lokacin tsarin tsufa, wanda ke ƙara yawan haɗin haɗin gwiwa, kuma ƙarfin ƙarfin duk rubbers yana ƙaruwa bayan tsufa, yana nuna cewa HNBR yana da kyawawan kaddarorin zafin jiki. Bugu da ƙari, ƙari na zinc oxide da magnesium oxide sun inganta sosai

Bugu da kari, da zinc oxide da magnesium oxide iya muhimmanci inganta kudi na canji na tensile elongation bayan zafi juriya, da kuma kudi na canji na tensile elongation na roba abu ragewa tare da karuwa da sashi na kayan, wanda ya nuna m high-zazzabi juriya, wanda za a iya dangana ga gaskiyar cewa karfe oxides kansu na cikin thermal oxides da kansu na cikin thermally ƙetare da rubber abun da ke ciki na iya kara yawan ƙetare abubuwan da rubber. hana harin sarkar oxygen na kwayoyin halitta, da inganta yanayin juriya mai zafi na kayan roba. A lokaci guda, ƙari na zinc oxide na iya rage raguwa na dindindin na lalata na roba, amma tare da adadinsa ba ya canzawa sosai; magnesium oxide akan matsawa nakasawa na dindindin na tasiri ba shi da mahimmanci. Sabili da haka, ƙara yawan adadin ƙarfe mai dacewa a cikin tsarin vulcanization na peroxide yana taimakawa wajen inganta yanayin zafi na roba.

 

Lokacin da adadin zinc oxide ya kasance sassa 5, TG-DTG curve na kayan roba na HNBR, irin su bazuwar thermal na kayan roba ya bayyana matakai biyu a bayyane, wanda galibi saboda ƙungiyoyi daban-daban na HNBR sarkar ƙwayoyin cuta zazzabi ya bambanta. Matakin farko shine butyl

Mataki na farko da aka yafi lalacewa ta hanyar thermal cleavage na biyu bond a butadiene, da kuma na biyu mataki ne ya sa ta cyclization na acrylonitrile sarkar sashi a lokacin dumama tsari don samar da wani chelate fili, wanda za a iya kawai cleaved a wani sosai high zafin jiki , don haka akwai biyu bayyananne thermal cleavage matakan, da kuma na 4 rubber matsakaicin adadin zafin jiki ya bayyana. 4 , wanda ke nuna babban kwanciyar hankali na thermal.

 

Na farko thermal bazuwar zafin jiki (lokacin da taro asarar kudi ne 5%) da kuma matsakaicin bazuwar rate zafin jiki na roba abu da m iri daya Trend, da Bugu da kari na karfe oxides iya rage matsakaicin taro asarar kudi na  roba abu, a cikin abin da na farko thermal bazuwar zafin jiki na 5 sassa na zinc oxide roba abu ne ya karu da kusan 15 ℃. na zinc oxide na iya rubber rubber, wanda 5 inganta ingantaccen yanayin zafi na kayan roba, amma lokacin da adadin zinc oxide ya kasance sassa 10, bazuwar thermal na farko Duk da haka, lokacin da adadin zinc oxide ya kasance sassa 10, farkon yanayin bazuwar thermal ya ragu. Wannan na iya zama saboda: (1) rashin tarwatsawar zinc oxide; (2) zinc oxide da yawa a cikin tsarin vulcanization na peroxide ya haifar da haɗin haɗin giciye yana cutar da kwanciyar hankali na thermal. Dalilin da ya sa wannan ya rage don ƙarin bincike. An rage yawan zafin jiki na farko na zafin jiki na 5-sashe na magnesium oxide rubber abu idan aka kwatanta da abin da ba a sani ba, kuma za a iya ƙara yawan zafin jiki na zafin jiki na kayan roba kawai lokacin da adadin magnesium oxide ya kasance sassa 10. Yin amfani da bincike na TG don nuna yanayin juriya na roba na silicone, sakamakon ya nuna cewa zafin iska na tsufa na silicone roba da zafin jiki na bazuwar zafin jiki a cikin yanayin iskar oxygen na yanayin canjin ya fi daidaituwa, amma a cikin wannan gwajin su biyun ba su samar da wani takamaiman wasiƙa ba, amma matsakaicin adadin asarar taro da yanayin canji a cikin aikin zafin iska mai zafi yana iya zama mafi daidaituwa ga nau'ikan nau'ikan nau'ikan nau'ikan nau'ikan nau'ikan nau'ikan nau'ikan nau'ikan nau'ikan nau'ikan rubber. nau'ikan bazuwar thermal daban-daban da kuma nazarin TG na yanayi (kamar yanayin iskar gas). Wannan na iya zama saboda bambance-bambance a cikin na'urar bazuwar thermal na nau'ikan roba daban-daban da yanayi daban-daban na bincike na TG (misali yanayin iskar gas), don haka idan ana amfani da bincike na TG don kimanta juriyar tsufa na iska mai zafi na roba, ainihin tsari da yanayin gwaji yakamata a yi la'akari da su sosai.

 

2. zinc oxide / magnesium oxide da kuma amfani da adhesives a kan zafi da iska tsufa juriya da matsawa m nakasawa sakamako.

Lokacin da rabo na zinc oxide / magnesium oxide shine 7/3, akwai tasiri mai tasiri akan aikin tsufa na iska mai zafi na m, kuma manne yana da mafi kyawun juriya na zafi, yayin da ƙari na magnesium oxide yana da mummunan tasiri akan matsawa na dindindin nakasar juriya na m.

 

Kammalawa

(1) Bugu da kari na zinc oxide ko magnesium oxide a cikin HNBR peroxide vulcanization tsarin na iya haifar da kunnawa sakamako a kan roba abu da kuma inganta mataki na crosslinking na roba abu, da kuma aiki na zinc oxide ne mafi girma fiye da na magnesium oxide, da kuma mataki na crosslinking na roba abu yana nuna wani sama Trend tare da karuwa da ta rage adadin shi ne sakamakon oxides, amma a lokacin da oxide na iya haifar da karuwa a cikin adadin 10. na yawan damuwa na yau da kullum saboda mummunan tarwatsawa, amma yawan ruwa na kayan roba ya lalace, wanda ba shi da tasiri a kan darajar sake dawowa da juriya na abrasion. Juriyar abrasion yana da ɗan tasiri.

(2) Yin amfani da zinc oxide guda ɗaya ko magnesium oxide na iya inganta haɓakar zafi da juriya na tsufa na peroxide vulcanized HNBR mahadi, kuma tare da haɓaka yawan juriya na zafi, juriya mai zafi da juriya na abrasion.

Adadin juriya na zafi yana ƙaruwa, yayin da ƙari na zinc oxide zai iya haɓaka juriya na nakasawa na dindindin na roba, yayin da magnesium oxide yana da ɗan tasiri akansa.

(3) Bazuwar thermal na roba na HNBR yana cikin matakai biyu, ƙari na ƙarfe oxides na iya rage matsakaicin adadin asarar taro, sassan 5 na zinc oxide na iya inganta ingantaccen kwanciyar hankali na roba.

(4) Lokacin da zinc oxide / magnesium oxide da rabo na 7/3, mafi kyawun juriya na zafi na roba, amma magnesium oxide yana da mummunan tasiri akan juriya na roba don matsawa nakasar dindindin.


SAUKAR HANYA

KAYANMU

BAYANIN HULDA

Ƙara: No.33, Lane 159, Taiye Road, Fengxian District, Shanghai
Tel / WhatsApp / Skype: +86 15221953351
Haƙƙin mallaka     2023 Shanghai Herchy Rubber Co., Ltd. Taswirar yanar gizo |   Manufar Keɓantawa | Taimako Ta Leadong.