Ku langutiwa: 0     Mutsari: Muhleri ​​wa Sayiti Nkarhi wo kandziyisa: 2023-08-15 Masungulo: Ndhawu

Vutisa

Tanihi xin’wana xa switirhisiwa swosungula leswi tirhisiwaka eka bindzu ra rhaba, ntirho wa zinc oxide awu cinca hiku hluvukisiwa ka thekinoloji ya rhaba.

Kusuka eka xitirhisiwa xosungula xo penda, xitirhisiwa xo tiyisisa kuya eka sisiteme ya vulcanization xinga pfuxeta nkarhi wa vulcanization wa xiaki lexi tirhaka, rhaba ya chloroprene na rhaba ya carboxy eka xiaki xa vulcanizing, swiyimo swa dynamic swa switirhisiwa swa rhaba leswi tirhisiwaka eka thermal conductivity ya filler, na swin’wana, leswi tani hi sisiteme ya vulcanization ya xitirhisiwa lexi tirhaka, zinc oxide yahari muxaka lowu tirhaka swinene wa swilo. Magnesium oxide yinga tlhela yitirhisiwa tani hi xitirhisiwa lexi tirhaka eka vulcanization ya rhaba, kambe hikokwalaho ka ntirho wale hansi xikan’we na swivumbeko swa physical swa material ya rhaba ayi kahle, hikokwalaho magnesium oxide yitirhisiwa ngopfu tani hi vulcanizing agent xikan’we na heat stabilizer eka rhaba leyingana halogen.

 

Peroxide vulcanization i peroxide na rhaba eka maendlelo ya vulcanization swihumelela free radical addition reaction kuva yi endla bond yale henhla ya bond energy cc bond.

Loko yi pimanyisiwa na sulphur yellow vulcanization, yina swipfuno swaku tiya kahle ka kuhisa, matirhelo ya kahle swinene ya compression permanent deformation, ayi olovi ku fafazela xirhami, na nhlanganiso wo olova, etc. Emalembeni ya sweswinyana, yitirhisiwile ngopfu eka switirhisiwa swa rhaba ehansi ka swiyimo swa mahiselo yale henhla. Kusuka eka cross-linking mechanism, peroxide vulcanization system ayi nge tirhisiwi hi ti metal oxides, kambe eka maendlelo ya xiviri ya vuhumelerisi, vanhu vaha tala ku engetela kwalomu ka 5 wa swiphemu swa ti metal oxides eka formula, na kutirhisiwa ka yona hiku kongoma ka mbuyelo wa mavonelo yohambana hambana. Dyondzo yikombisa leswaku nano zinc oxide, magnesium oxide, calcium oxide na unsaturated acid swinga tirhisiwa tani hi co-crosslinking agent leyintshwa eka peroxide vulcanized hydrogenated nitrile butadiene rubber (HNBR), leswinga hungutaka nkarhi wa vulcanization naku antswisa crosslink density xikan’we na swivumbeko swa physical, kambe mbuyelo eka ku tiya ka kuhisa ka rhaba aswi boxiwanga.

 

1. Vuyelo bya zinc oxide kumbe magnesium oxide eka swivumbeko swa swilo swa rhaba

Loko ku pimanyisiwa na xikombiso xa blank, ku engeteriwa ka zinc oxide kumbe magnesium oxide rubber M swi engetelekile, naswona zinc oxide rubber ML yi le henhla, leswi swivangiwa hi zinc oxide yina ndzhawu leyikulu yale henhla xikan’we na mbuyelo wo tiya wa interfacial, eka matrix ya rhaba ayi olovi ku hangalasa, ya olova kuva yi hlanganisiwa, agglomeration, leswi endlaka leswaku rubber ML yi engeteleka, yikahle ku khuluka ka mati. Ku engeteriwa ka ti metal oxides switlhela swi engetela MH-ML ya compound, leswi kombaka leswaku ti metal oxides tinga hlohletela crosslinking, ti antswisa degree ya vulcanization, kambe titlhela ti pfuxeta T10 kambe tina mbuyelo wutsongo eka T90. Ku engetela kwalano, MH-ML ya ti zinc oxide compounds ayiri e henhla kutlula ya ti magnesium oxide compounds eka mpimo lowu fanaka, leswi kombisaka leswaku zinc oxide yina mbuyelo lowukulu wo activating eka vulcanization kutlula magnesium oxide eka peroxide vulcanization system.

 

Hiku tlakuka ka zinc oxide na magnesium oxide dosage, tensile strength ya vulcanized rubber ya sungula ku tlakuka kutani ya hunguteka, 100% constant elongation stress hiku angarhela yitala ku tlakuka, kasi elongation eka break and tear strength i trend leyi hungutaka, naswona eka dosage leyi fanaka ya zinc oxide rubber material constant elongation stress yile henhla kutlula magnesium oxide rubber material, leswi swifana na swihlawulekisi swa vulcanization swa MH-ML trend, kambe loko mpimo wa zinc oxide wuri 10 wa swiphemu swa 100% constant elongation stress ya vulcanized rubber i trend leyi hungutaka, leswinga vangiwa hiku hangalaka lokunga kahle ka zinc oxide. Hambiswiritano, loko mpimo wa zinc oxide wuri 10 wa swiphemu, 100% constant elongation stress ya vulcanized rubber yikombe kuhunguteka ka ntshamiseko, leswinga vangiwa hiku hangalaka kahle ka zinc oxide. Hiku komisa, ku engeteriwa ka ti metal oxides swinga antswisa crosslinking density ya rhaba ya HNBR ehansi ka peroxide vulcanization system, naswona degree ya crosslinking ya rhaba leyingana zinc oxide yile henhla kutlula ya magnesium oxide ehansi ka mpimo lowu fanaka, kambe loko mpimo wa zinc oxide wuri 10 wa swiphemu swa ku hangalaka lokunga cinciki, leswi endlaka leswaku kuva na kuhunguteka ka constant ntshikelelo wa ku leha. Kusuka eka Tafula ra 2, swinga tlhela swi voniwa leswaku ku engeteriwa ka ti oxides ta nsimbi swinga antswisa ku tiya, kambe hi mpimo wa yona aswi cinci ngopfu, naswona mbuyelo eka nkoka wa rebound awuri wa nkoka, laha mpimo wa zinc oxide wunga na mbuyelo lowukulu eka DIN abrasion, magnesium oxide vulcanized adhesive abrasion na mpimo wa yona wu tlakuka naswona wutala ku tlakuka, kambe abrasion hinkwayo yahari eka levele yale hansi, leyi nakambe yi kombisa hi ku hetiseka leswaku xinamarheti xa HNBR xi na ku tiya ka kahle swinene ka ku rhurhumela.

 

Ku dyuhala ka HNBR i ka muxaka wa chain cross-linking, leswi vonakaka hikuhunguteka ka tensile elongation xikan’we naku tlakuka ka hardness na tensile strength endzhaku ka ku dyuhala. Leswi swikomba leswaku cross-linking reaction yiya emahlweni hinkarhi wa maendlelo ya ku dyuhala, leswi engetelaka cross-linking density, naswona matimba ya tensile ya ti rhaba hinkwato ya tlakuka endzhaku ka ku dyuhala, leswi kombaka leswaku HNBR yina swivumbeko swa kahle swinene swa high temperature tensile. Ku engetela kwalaho, ku engeteriwa ka zinc oxide na magnesium oxide swi antswise swinene...

Ku engetela kwalano, ku engeteriwa ka zinc oxide na magnesium oxide swinga antswisa swinene mpimo wa ku cinca ka tensile elongation endzhaku ka ku tiya ka kuhisa, naswona mpimo wa ku cinca ka tensile elongation ya xitirhisiwa xa rhaba wuhunguteka loko ku tlakuka mpimo wa swilo leswi, leswi kombisaka ku tiya ka kahle swinene ka mahiselo yale henhla, leswinga vangiwa hi mhaka ya leswaku ti oxides ta nsimbi hi toxe ti wela eka swilo leswi tiyeke hi mahiselo naswona tinga engeteleka cross-linking density ya swilo swa rhaba, leswinga yaka emahlweni swi sivela nhlaselo wa molecular chain ya oxygen, naku antswisa matirhelo ya high-temperature resistance ya xitirhisiwa xa rhaba. Hi nkarhi lowu fanaka, ku engeteriwa ka zinc oxide swinga hunguta swinene compression permanent deformation ya rhaba, kambe hi mpimo wa yona awu cinci ngopfu; magnesium oxide eka compression permanent deformation ya nkucetelo a yi na nkoka ngopfu. Hikokwalaho, ku engeteriwa ka nhlayo leyi faneleke ya ti metal oxides eka peroxide vulcanization system swi pfuneta ku antswisa ku tiya ka kuhisa ka rhaba.

 

Loko mpimo wa zinc oxide wuri 5 wa swiphemu, TG-DTG curve ya HNBR rabber material, kufana na thermal decomposition ya rhaba material yivonile swiri erivaleni swinene switeji swimbirhi, leswi ngopfu ngopfu swivangiwa hi mintlawa yimbirhi yohambana ya HNBR molecular chain decomposition temperature ya hambanile. Xiyenge xosungula ngopfu ngopfu i butyl

Xiyenge xosungula xivangiwa ngopfu hiku hambanisiwa ka mahiselo ya double bond eka butadiene, naswona xiteji xavumbirhi xivangiwa hiku cyclization ka xiphemu xa acrylonitrile chain hi nkarhi wa maendlelo yo hisa kuva xi endla chelate compound, leyinga hambanisiwaka ntsena eka mahiselo yale henhla swinene , hikokwalaho kuna switeji swimbirhi leswinga erivaleni swa thermal cleavage, naswona mahiselo yale henhla ya ku bola ka swilo swa rhaba leswi humeleleke eka 468.49 °C , leswi kombisaka ku tiya ka mahiselo yale henhla.

 

Mahiselo yosungula ya ku bola hi mahiselo (loko mpimo wa ku lahlekeriwa hi vukulu yiri 5%) xikan’we na mahiselo yale henhla ya mpimo wa ku bola ka swilo swa rhaba hi xisekelo swina ntshamiseko lowu fanaka, naswona ku engeteriwa ka ti oxides ta nsimbi swinga hunguta mpimo lowukulu wa ku lahlekeriwa hi vukulu bya  swilo swa rhaba, laha mahiselo yosungula ya ku bola ka mahiselo ya 5 wa swiphemu swa swilo swa rhaba ya zinc oxide ya engeteriwaka kwalomu ka 15 °C loko ku pimanyisiwa na ya rhaba leyi nga riki na nchumu material, leswi kombisaka leswaku swiphemu swa 5 swa zinc oxide swinga antswisa swinene ku tiya ka mahiselo ya material ya rhaba, kambe loko mpimo wa zinc oxide wuri 10 wa swiphemu, ku bola kosungula ka mahiselo Kambe loko mpimo wa zinc oxide wuri 10 wa swiphemu, mahiselo yosungula ya ku bola ka mahiselo ya hungutekile. Leswi swi nga ha va swi vangiwa hi: (1) ku hangalaka loku nga riki kahle ka zinc oxide; (2) zinc oxide yotala swinene eka peroxide vulcanization system yi humese ti cross-linking bonds leti onhaka eka ku tiya ka mahiselo. Xivangelo lexi kongomeke xa leswi xa ha fanele ku lavisisiwa ku ya emahlweni.Mahiselo yosungula ya ku bola ka mahiselo ya 5-part magnesium oxide rubber material ya hungutiwile loko ya pimanyisiwa na ya blank rubber material, naswona mahiselo ya thermal decomposition ya rhaba material yanga engeteriwa ntsena loko nhlayo ya magnesium oxide yiri 10 wa swiphemu. Ku tirhisiwa ka nxopaxopo wa TG ku hlamusela ku tiya ka ku hisa ka rhaba ya silicone, mbuyelo wu kombisa leswaku matirhelo ya ku dyuhala ka moya wo hisa wa rhaba ya silicone na mahiselo ya ku bola hi ku hisa eka xibakabaka xa okisijini ya ntshamiseko wa ku cinca swi tshamisekile swinene, kambe eka xikambelo lexi leswimbirhi a swi vumbanga ku yelana ko karhi, kambe ku tlula kwalaho i mpimo lowukulu wa ku lahlekeriwa hi vukulu naswona ntshamiseko wa ku cinca eka matirhelo ya ku hisa ka moya wo hisa wu tshamisekile swinene, leswi nga ha vaka ku va hikwalaho ka ku bola hi ku hisa ka tinxaka to hambana ta rhaba na endlelo ro hambana ra ku bola hi ku hisa na nxopaxopo wa TG wa swiyimo (ku fana na xibakabaka xa gasi). Leswi swinga vangiwa hiku hambana eka endlelo ro bola hi mahiselo ya tinxaka tohambana hambana ta rhaba xikan’we na swiyimo swohambana hambana swa nxopaxopo wa TG (xikombiso xibakabaka xa gasi), hikokwalaho loko nxopaxopo wa TG wutirhisiwa ku kambela ku lwisana ka ku dyuhala ka moya wo hisa ka rhaba, ku endliwa ka xiviri na swiyimo swa xikambelo swifanele ku tekeriwa enhlokweni hiku hetiseka.

 

2. zinc oxide / magnesium oxide na ku tirhisiwa ka swinamarheti eka ku hisa na moya ku lwisana na ku dyuhala na compression permanent deformation effect

Loko ratio ya zinc oxide/magnesium oxide yiri 7/3, kuna mbuyelo wa synergistic eka matirhelo ya ku dyuhala ka moya wo hisa wa adhesive, naswona adhesive yina ku tiya lokunene ka kuhisa, kasi ku engeteriwa ka magnesium oxide swina mbuyelo wo biha eka compression permanent deformation resistance ya adhesive.

 

Mahetelelo

(1) )Ku engeteriwa ka zinc oxide kumbe magnesium oxide eka sisiteme ya HNBR peroxide vulcanization swi nga humesa mbuyelo wa activation eka swilo swa rhaba na ku antswisa mpimo wa ku hlanganisiwa ka swilo swa rhaba, naswona ntirho wa zinc oxide wu le henhla ku tlula wa magnesium oxide, naswona mpimo wa ku hlanganisiwa ka swilo swa rhaba wu kombisa ntshamiseko wo ya ehenhla hi ku tlakuka ka mpimo wa wona, kambe loko nhlayo ya zinc oxide i 10 wa swiphemu, swinga endla leswaku kuva na kuhunguteka ka constant tensile stress hikokwalaho ka ku hangalaka lokunga kahle, kambe fluidity ya rubber material ya onhaka, leswinga na mbuyelo wutsongo eka rebound value xikan’we na abrasion resistance. Ku lwisana na ku rhurhumela a ku na vuyelo byintsongo.

(2) Ku tirhisiwa kan’we ka zinc oxide kumbe magnesium oxide swi nga antswisa swinene ku tiya ka ku hisa na ku dyuhala ka moya ka swihlanganisi swa HNBR leswi endliweke hi peroxide vulcanized, naswona hi ku tlakuka ka nhlayo ya ku lwisana na ku hisa, ku lwisana na ku hisa na ku lwisana na ku rhurhumela.

Nhlayo ya ku tiya ka kuhisa ya tlakuka, kasi ku engeteriwa ka zinc oxide swinga antswisa ku tiya ka compression permanent deformation ya rhaba, kasi magnesium oxide ayi na mbuyelo wutsongo eka yona.

(3)Ku bola hi ku hisa ka rhaba ya HNBR ku le ka switeji swimbirhi, ku engeteriwa ka ti-oxide ta nsimbi swi nga hunguta mpimo lowukulu wa ku lahlekeriwa hi vukulu, swiphemu swa 5 swa zinc oxide swi nga antswisa swinene ku tiya ka ku hisa ka rhaba.

(4) Loko zinc oxide / magnesium oxide na ratio ya 7 / 3, ku tiya lokunene ka ku hisa ka rhaba, kambe magnesium oxide yi na nkucetelo wo biha eka ku lwisana ka rhaba eka compression permanent deformation performance.


XITLHOKOVETSELO XA XITLHANYI

SWILO SWA HINA

VUXOKOXOKO BYA VUXOKOXOKO

Engetelani: No.33, Lane 159, Gondzo ra Taiye, Xifundzha xa Fengxian, Shanghai
Riqingho / WhatsApp / Skype: +86 15221953351
Vukorhokeri bya Vutshila     2023 Shanghai Herchy Rubber Co., Ltd. Mepe wa sayiti |   Pholisi ya Vuhlayiseki | Nseketelo Hi Leadong.