Tel: +86 15221953351 E-mail: info@herchyrubber.com
Please Choose Your Language
Xov xwm
Koj tseem nyob ntawm no: Tsev » Xov xwm » Xov xwm » Cov nyhuv ntawm zinc oxide thiab magnesium oxide ntawm cov khoom ntawm peroxide vulcanized HNBR

Cov nyhuv ntawm zinc oxide thiab magnesium oxide ntawm cov khoom ntawm peroxide vulcanized HNBR

Views: 0     Author: Site Editor Publish Time: 2023-08-15 Keeb Kwm: Qhov chaw

Nug

Raws li ib qho ntawm cov ntaub ntawv ntxov tshaj plaws siv hauv kev lag luam roj hmab, lub luag haujlwm ntawm zinc oxide tau hloov nrog kev txhim kho cov cuab yeej siv roj hmab.

Los ntawm thawj xim tus neeg sawv cev, tus neeg sawv cev txhawb zog rau lub vulcanization system tuaj yeem ua kom luv luv lub sij hawm vulcanization ntawm tus neeg sawv cev nquag, chloroprene roj hmab thiab carboxy roj hmab hauv tus neeg sawv cev vulcanizing, dynamic tej yam kev mob ntawm cov khoom siv roj hmab siv nyob rau hauv thermal conductivity ntawm cov muab tub lim, thiab lwm yam. Magnesium oxide kuj tseem siv tau los ua tus neeg sawv cev ua haujlwm hauv vulcanization ntawm roj hmab, tab sis vim tias qhov kev ua haujlwm qis dua thiab lub cev ntawm cov khoom siv roj hmab tsis zoo, yog li magnesium oxide feem ntau yog siv los ua tus neeg sawv cev vulcanizing thiab kub stabilizer hauv halogen roj hmab.

 

Peroxide vulcanization yog peroxide thiab roj hmab hauv cov txheej txheem vulcanization tshwm sim dawb radical ntxiv cov tshuaj tiv thaiv los tsim ib daim ntawv cog lus siab zog cc.

Piv nrog sulfur yellow vulcanization, nws muaj qhov zoo ntawm kev ua kom sov zoo, zoo heev compression mus tas li deformation kev ua tau zoo, tsis yooj yim rau tshuaj tsuag Frost, thiab kev sib koom ua ke yooj yim, thiab lwm yam. Nyob rau hauv xyoo tas los no, nws tau siv dav hauv cov khoom siv roj hmab nyob rau hauv qhov kub thiab txias. Los ntawm kev sib txuas ntawm cov txheej txheem, peroxide vulcanization system tsis tuaj yeem qhib los ntawm cov hlau oxides, tab sis nyob rau hauv cov txheej txheem tsim tawm tiag tiag, tib neeg tseem feem ntau ntxiv txog 5 feem ntawm cov hlau oxides hauv cov mis, thiab nws cov kev siv tshwj xeeb ntawm cov nyhuv ntawm cov kev xav sib txawv. Txoj kev tshawb no qhia tau hais tias nano zinc oxide, magnesium oxide, calcium oxide thiab unsaturated acid yuav siv tau raws li ib tug tshiab co-crosslinking tus neeg sawv cev nyob rau hauv peroxide vulcanized hydrogenated nitrile butadiene roj hmab (HNBR), uas yuav txo tau lub sij hawm vulcanization thiab txhim kho crosslink ceev thiab lub cev zog, tab sis cov nyhuv ntawm lub tshav kub tsis kam ntawm cov roj hmab tsis tau hais.

 

1. Cov nyhuv ntawm zinc oxide lossis magnesium oxide ntawm cov khoom ntawm cov khoom siv roj hmab

Piv nrog rau cov qauv dawb paug, qhov sib ntxiv ntawm zinc oxide lossis magnesium oxide roj hmab M tau nce, thiab zinc oxide roj hmab ML yog siab dua, qhov no yog vim zinc oxide muaj thaj tsam loj dua thiab muaj zog cuam tshuam, hauv cov roj hmab matrix tsis yooj yim tawg, yooj yim rau cohesion, agglomeration, uas ua rau cov roj hmab ML nce, dej tsis zoo. Qhov sib ntxiv ntawm cov hlau oxides kuj ua rau MH-ML ntawm cov khoom sib xyaw ua ke, uas qhia tau tias cov hlau oxides tuaj yeem txhawb kev sib txuas, txhim kho qib ntawm vulcanization, tab sis kuj txo T10 tab sis muaj kev cuam tshuam me ntsis ntawm T90. Tsis tas li ntawd, MH-ML ntawm zinc oxide tebchaw yog siab dua li ntawm magnesium oxide tebchaw nyob rau tib qhov ntau npaum li cas, uas qhia tau hais tias zinc oxide muaj kev ua kom muaj zog ntawm vulcanization ntau dua li magnesium oxide nyob rau hauv peroxide vulcanization system.

 

Nrog rau qhov nce ntawm zinc oxide thiab magnesium oxide ntau npaum li cas, lub zog tensile ntawm vulcanized roj hmab thawj zaug nce thiab tom qab ntawd txo qis, 100% tas li elongation kev ntxhov siab tag nrho yuav nce ntxiv, thaum lub elongation ntawm tawg thiab tsim kua muag lub zog yog ib qho kev txo qis, thiab tib lub zog ntawm zinc oxide roj hmab cov khoom siv tas li cov khoom siv elongation yog siab dua li magnesium vulcanization. MH-ML sib txawv, tab sis thaum noj zinc oxide yog 10 feem ntawm 100% tas li elongation kev ntxhov siab ntawm vulcanized roj hmab yog ib qho kev poob qis, uas tej zaum yuav tshwm sim los ntawm kev tsis zoo ntawm zinc oxide dispersion. Txawm li cas los xij, thaum qhov ntau npaum ntawm zinc oxide yog 10 feem, 100% tas li elongation kev ntxhov siab ntawm cov roj hmab vulcanized pom qhov txo qis, uas yuav tshwm sim los ntawm kev tsis zoo ntawm zinc oxide dispersion. Hauv cov ntsiab lus, qhov sib ntxiv ntawm cov hlau oxide tuaj yeem txhim kho qhov sib txawv ntawm HNBR roj hmab hauv qab peroxide vulcanization system, thiab cov qib crosslinking ntawm zinc oxide-muaj roj hmab yog siab dua li ntawm magnesium oxide nyob rau hauv tib qhov ntau npaum li cas, tab sis thaum noj zinc oxide yog 10 feem ntawm cov neeg pluag dispersion, uas ua rau txo qis ntawm kev ntxhov siab. Los ntawm Table 2, nws tseem tuaj yeem pom tias qhov sib ntxiv ntawm cov hlau oxide tuaj yeem txhim kho qhov nyuaj, tab sis nrog nws cov tshuaj tsis hloov ntau, thiab cov txiaj ntsig ntawm tus nqi rov qab tsis tseem ceeb, uas cov zinc oxide ntau npaum li cas tsis muaj qhov cuam tshuam loj rau DIN abrasion, magnesium oxide vulcanized adhesive abrasion nrog nws qhov ntau npaum li cas nce thiab txo qis dua, tab sis kuj tseem nce ntxiv, qhia tau hais tias HNBR nplaum muaj qhov ua tau zoo heev.

 

Kev laus ntawm HNBR belongs rau cov saw cross-linking hom, uas yog manifested nyob rau hauv qhov txo ntawm tensile elongation thiab nce hardness thiab tensile zog tom qab laus. Qhov no qhia tau hais tias qhov kev sib txuas txuas txuas ntxiv txuas ntxiv thaum lub sijhawm kev laus, uas ua rau muaj kev sib txuas ntawm qhov sib txuas, thiab lub zog tensile ntawm tag nrho cov roj hmab nce tom qab kev laus, qhia tias HNBR muaj qhov zoo ntawm qhov kub thiab txias tensile zog. Tsis tas li ntawd, qhov sib ntxiv ntawm zinc oxide thiab magnesium oxide ua kom zoo dua qub

Tsis tas li ntawd, qhov sib ntxiv ntawm zinc oxide thiab magnesium oxide tuaj yeem txhim kho tus nqi ntawm kev hloov ntawm tensile elongation tom qab tshav kub, thiab qhov kev hloov ntawm tensile elongation ntawm cov khoom siv roj hmab txo qis nrog qhov nce ntawm cov khoom siv, uas qhia tau hais tias zoo heev kub-kub kuj, uas tej zaum yuav raug ntaus nqi mus rau lub fact tias hlau oxides lawv tus kheej muaj nyob rau hauv lub thermally elongation ntawm cov ntaub ntawv uas muaj peev xwm mus txuas ntxiv stability ntawm cov khoom. cuam tshuam qhov kev tawm tsam ntawm cov saw hlau molecular ntawm cov pa oxygen, thiab txhim kho qhov kub thiab txias ua haujlwm ntawm cov khoom siv roj hmab. Nyob rau tib lub sijhawm, qhov sib ntxiv ntawm zinc oxide tuaj yeem txo qhov compression mus tas li deformation ntawm cov roj hmab, tab sis nrog nws qhov ntau npaum li cas tsis hloov ntau; magnesium oxide ntawm compression mus tas li deformation ntawm qhov cuam tshuam tsis tseem ceeb heev. Yog li ntawd, qhov sib ntxiv ntawm qhov tsim nyog ntawm cov hlau oxides nyob rau hauv peroxide vulcanization system pab txhim kho cov cua sov ntawm cov roj hmab.

 

Thaum qhov ntau npaum ntawm zinc oxide yog 5 qhov chaw, TG-DTG nkhaus ntawm HNBR cov khoom siv roj hmab, xws li thermal decomposition ntawm cov khoom siv roj hmab tau tshwm sim ob theem, uas yog vim yog ob pawg sib txawv ntawm HNBR molecular saw decomposition kub yog txawv. Thawj theem yog cov butyl

Thawj theem yog tshwm sim los ntawm thermal cleavage ntawm ob daim ntawv cog lus nyob rau hauv butadiene, thiab lub thib ob theem yog tshwm sim los ntawm lub cyclization ntawm lub acrylonitrile saw segment thaum lub sij hawm cua sov txheej txheem los ua ib tug chelate compound, uas tsuas yog cleaved ntawm ib tug kub heev, yog li ntawd muaj ob pom tseeb thermal cleavage theem, thiab lub siab tshaj plaws decomposition kub ntawm 4 6. ruaj khov.

 

Thawj thermal decomposition kub (thaum lub loj poob tus nqi yog 5%) thiab lub siab tshaj plaws decomposition tus nqi kub ntawm cov khoom siv roj hmab muaj ib tug zoo sib xws, thiab ntxiv cov hlau oxides yuav txo tau qhov siab tshaj plaws poob tus nqi ntawm cov  khoom siv roj hmab, nyob rau hauv uas thawj thermal decomposition kub ntawm 5 qhov chaw ntawm zinc oxide roj hmab cov ntaub ntawv yog nce los ntawm ze li ntawm 15 ℃ piv nrog cov oxide ntawm cov roj hmab tseem ceeb ntawm oxide 5. cov khoom siv roj hmab, tab sis thaum noj zinc oxide yog 10 feem, qhov pib thermal decomposition Txawm li cas los xij, thaum qhov ntau npaum ntawm zinc oxide yog 10 feem, qhov pib thermal decomposition kub poob. Qhov no tej zaum yuav yog vim: (1) tsis zoo dispersion ntawm zinc oxide; (2) ntau zinc oxide nyob rau hauv lub peroxide vulcanization system ua cross-linking bonds detrimental rau lub thermal stability. Qhov laj thawj tseem ceeb ntawm qhov no tseem yuav tsum tau tshawb xyuas ntxiv.Qhov pib thermal decomposition kub ntawm 5 feem ntawm magnesium oxide roj hmab cov khoom raug txo qis piv rau cov khoom siv roj hmab dawb, thiab cov thermal decomposition kub ntawm cov khoom siv roj hmab tsuas yog nce thaum cov nyiaj magnesium oxide yog 10 feem. Kev siv TG tsom xam cov yam ntxwv ntawm cov cua sov ua haujlwm ntawm silicone roj hmab, cov txiaj ntsig tau pom tias cov cua kub cua aging kev ua tau zoo ntawm silicone roj hmab thiab cov thermal decomposition kub nyob rau hauv cov pa oxygen ntawm qhov kev hloov ntawm qhov sib txawv ntawm qhov sib txawv, tab sis nyob rau hauv qhov kev ntsuam xyuas no ob tsis tau tsim ib qho kev sib txuas lus, tab sis yog qhov siab tshaj plaws ntawm huab cua poob thiab qhov sib txawv ntawm kev hloov pauv hauv kev ua tau zoo ntawm cov cua kub cua aging yog qhov sib txawv ntawm qhov sib txawv ntawm qhov sib txawv, uas tej zaum yuav txawv. decomposition mechanism thiab TG tsom xam ntawm tej yam kev mob (xws li roj cua). Qhov no tej zaum yuav yog vim qhov sib txawv ntawm cov thermal decomposition mechanism ntawm cov roj hmab sib txawv thiab cov kev mob sib txawv ntawm TG tsom xam (xws li roj cua), yog li yog tias TG tsom xam siv los ntsuas qhov kub ntawm huab cua aging kuj ntawm cov roj hmab, qhov tseeb formulation thiab kuaj tej yam kev mob yuav tsum tau txiav txim siab comprehensively.

 

2. zinc oxide / magnesium oxide thiab kev siv cov nplaum rau ntawm cov cua sov thiab huab cua aging kuj thiab compression mus tas li deformation nyhuv

Thaum qhov piv ntawm zinc oxide / magnesium oxide yog 7/3, muaj kev sib koom ua ke ntawm huab cua kub kev laus kev ua haujlwm ntawm cov nplaum, thiab cov nplaum muaj qhov ua kom sov zoo tshaj plaws, thaum ntxiv ntawm magnesium oxide muaj qhov tsis zoo ntawm compression mus tas li deformation tsis kam ntawm cov nplaum.

 

Xaus

(1)) Kev sib ntxiv ntawm zinc oxide lossis magnesium oxide hauv HNBR peroxide vulcanization system tuaj yeem tsim cov nyhuv ntawm cov khoom siv roj hmab thiab txhim kho qib ntawm kev sib txuas ntawm cov khoom siv roj hmab, thiab cov kev ua ntawm zinc oxide yog siab dua li ntawm magnesium oxide, thiab qib crosslinking ntawm cov khoom siv roj hmab qhia tau hais tias muaj kev nce siab ntxiv nrog kev nce ntawm nws qhov ntau npaum li cas, tab sis thaum qhov tshwm sim ntawm zinc oxide yog 10 constant oxide. tensile kev nyuaj siab vim tsis zoo dispersion, tab sis lub fluidity ntawm cov khoom siv roj hmab deteriorates, uas muaj me ntsis cuam tshuam rau tus nqi rebound thiab puas kuj. Abrasion kuj muaj me ntsis cuam tshuam.

(2) Kev siv ib leeg ntawm zinc oxide lossis magnesium oxide tuaj yeem txhim kho cov cua sov thiab huab cua aging kuj ntawm peroxide vulcanized HNBR tebchaw, thiab nrog rau qhov nce ntawm cov cua sov, tiv thaiv tshav kub thiab puas.

Tus nqi ntawm cov cua sov tuaj yeem nce ntxiv, thaum ntxiv zinc oxide tuaj yeem txhim kho cov compression mus tas li deformation tsis kam ntawm cov roj hmab, thaum magnesium oxide tsis tshua muaj txiaj ntsig rau nws.

(3) Lub thermal decomposition ntawm HNBR roj hmab yog nyob rau hauv ob theem, qhov sib ntxiv ntawm cov hlau oxides tuaj yeem txo qhov siab tshaj plaws ntawm cov khoom poob, 5 feem ntawm zinc oxide tuaj yeem txhim kho thermal stability ntawm cov roj hmab.

(4) Thaum zinc oxide / magnesium oxide thiab qhov sib piv ntawm 7 / 3, qhov zoo tshaj plaws tshav kub tsis kam ntawm cov roj hmab, tab sis cov magnesium oxide muaj kev cuam tshuam tsis zoo rau cov roj hmab tsis kam rau compression mus tas li deformation kev ua tau zoo.


QUICK LINKS

Peb cov khoom

Tiv tauj xov xwm

Ntxiv: No.33, Txoj Kev 159, Taiye Road, Fengxian District, Shanghai
Tel / WhatsApp / Skype: +86 15221953351
Copyright     2023 Shanghai Herchy Rubber Co., Ltd. Daim duab qhia chaw |   Txoj Cai Tswjfwm Ntiag Tug | Txhawb nqa By Leadong.