Views: 0 Author: Site Editor A chhuah hun: 2023-08-15 A chhuahna: Hmun
Rubber industry-a hmanraw hmasa ber zinga mi a nih angin, rubber technology lo chhuahnaah hian zinc oxide chanvo hi a danglam chho zel a ni.
A tir lama coloring agent atanga vulcanization system thlengin reinforcing agent hian active agent, vulcanizing agent-a chloroprene rubber leh carboxy rubber te vulcanization hun a ti tawi thei a, filler-a thermal conductivity-a hman rubber product-te dynamic conditions, etc., chu chu active agent vulcanization system angin zinc oxide hi material chi khat tangkai ber a la ni reng a ni. Magnesium oxide hi rubber vulcanization-ah pawh active agent atan hman theih a ni a, mahse a activity a hniam zawk avangin rubber material physical property a tha lo avangin magnesium oxide hi halogen awmna rubber-ah vulcanizing agent leh heat stabilizer atan hman a ni ber.
Peroxide vulcanization hi peroxide a ni a, vulcanization process-ah hian rubber chu free radical addition reaction a awm a, bond energy cc bond sang zawk a siam a ni.
Sulfur yellow vulcanization nena khaikhin chuan heat resistance tha tak, compression permanent deformation performance tha tak, frost spray awlsam lo, leh simple coordination, etc. a thatna a nei a, tun hnaiah rubber product-ah temperature sang tak hnuaiah hman a ni nasa hle. Cross-linking mechanism atang chuan peroxide vulcanization system hi metal oxide hian a tichak thei lo a, mahse a siam chhuah tak takah chuan miten formula-ah hian metal oxide hmun 5 vel an la dah fo thin a, a bik takin ngaihdan hrang hrangin nghawng a neih dan a hmang bawk. He zirchianna hian peroxide vulcanized hydrogenated nitrile butadiene rubber (HNBR)-ah nano zinc oxide, magnesium oxide, calcium oxide leh unsaturated acid te chu co-crosslinking agent thar atan hman theih a nih thu a tarlang a, hei hian vulcanization hun a ti tawi thei a, crosslink density leh physical property a ti tha thei a, mahse rubber hian heat resistance a nghawng dan erawh sawi a ni lo.
1. Zinc oxide emaw magnesium oxide emaw hian rubber material property a nghawng dan
Blank sample nen khaikhin chuan zinc oxide emaw magnesium oxide rubber M dah belh a ni a, zinc oxide rubber ML a sang zawk bawk a, hei hi zinc oxide hian surface area lian zawk leh interfacial effect chak tak a neih vang a ni a, rubber matrix-ah hian a darh awlsam lo va, cohesion a awlsam lo, agglomeration a awm a, chu chuan rubber ML a tipung a, a chhe hle fluidity (fluidity) a ni. Metal oxide dah belh hian compound MH-ML a tipung bawk a, hei hian metal oxide hian crosslinking a tichak thei a, vulcanization degree a ti tha thei a, mahse T10 a ti tawi thei a, mahse T90-ah erawh nghawng a nei tlem hle tih a tilang bawk. Tin, zinc oxide compound MH-ML chu magnesium oxide compound aiin a dose inangah a sang zawk a, hei hian peroxide vulcanization system-a magnesium oxide aiin zinc oxide hian vulcanization-ah activating effect nasa zawk a nei tih a tilang bawk.
Zinc oxide leh magnesium oxide dosage a san chuan vulcanized rubber tensile strength a sang hmasa a, chutah a tlahniam a, 100% constant elongation stress overall tendency chu a sang chho zel a, chutih laiin elongation at break and tear strength chu a tlahniam zel a, zinc oxide rubber material dosage inangah chuan magnesium oxide rubber aiin constant elongation stress a sang zawk bawk material, hei hi MH-ML trend-a vulcanization characteristics nen a inang a, mahse zinc oxide dosage chu vulcanized rubber 100% constant elongation stress hmun 10 a nih chuan a tlahniam zel a, hei hi zinc oxide dispersion tha lo vang a ni thei. Mahse, zinc oxide dosage chu part 10 a nih chuan vulcanized rubber-a 100% constant elongation stress chu tlahniam zel a ni a, hei hi zinc oxide dispersion tha lo vang a ni thei. A tawi zawngin, metal oxide dah belh hian peroxide vulcanization system hnuaia HNBR rubber crosslinking density a ti tha thei a, zinc oxide awmna rubber crosslinking degree chu magnesium oxide aiin a sang zawk a, mahse zinc oxide dosage chu poor dispersion portion 10 a nih chuan, chu chuan constant dispersion a tihhniam phah a ni elongation stress a ni. Table 2 atang hian metal oxide dah belh hian hardness a ti tha thei tih pawh a hriat theih a, mahse a dosage nen chuan a danglam vak lo va, rebound value-ah pawh nghawng a nei lian lo hle a, chutah chuan zinc oxide dosage hian DIN abrasion-ah nghawng lian tham a nei lo a, magnesium oxide vulcanized adhesive abrasion chu a dosage nen a pung a, a pung duh hle a, mahse abrasion pumpui chu a hniam zawk level-ah a la awm a, chu chu tin, HNBR adhesive hian abrasion resistance tha tak a nei tih a tilang chiang hle bawk.
HNBR tar chakna hi chain cross-linking type-ah a tel a, chu chu tensile elongation tlahniam leh tar hnua hardness leh tensile strength tihpunnaah a lang chhuak a ni. Hei hian aging process chhung hian cross-linking reaction a chhunzawm zel tih a tilang a, hei hian cross-linking density a tisang a, rubber zawng zawng tensile strength pawh a upa tawh hnuah a sang chho zel a, hei hian HNBR hian high temperature tensile property tha tak a nei tih a tilang a ni. Tin, zinc oxide leh magnesium oxide te dah belh hian nasa takin a tichangtlung a ni
Chu bakah, zinc oxide leh magnesium oxide dah belh hian heat resistance hnua tensile elongation inthlak dan rate nasa takin a ti tha thei a, rubber material-a tensile elongation inthlak dan rate pawh a tlahniam a, hei hian high-temperature resistance tha tak a lantir a, hei hi metal oxides ngei pawh hi thermally stable substance-a mi an nih vang a ni thei a, a pung thei bawk rubber material cross-linking density a awm a, hei hian oxygen molecular chain attack a tikhawtlai lehzual thei a, rubber material hian high-temperature resistance performance a ti tha thei bawk. Chutih rual chuan zinc oxide dah belh hian rubber-a compression permanent deformation chu nasa takin a tihtlem thei a, mahse a dosage nen chuan a danglam vak lo magnesium oxide chuan compression permanent deformation a nghawng nasa lutuk lo. Chuvangin, peroxide vulcanization system-ah hian metal oxide tling tawk dah belh hian rubber-in a lumna a do theihna tur a tichangtlung a ni.
Zinc oxide dosage chu part 5 a nih chuan HNBR rubber material TG-DTG curve, rubber material thermal decomposition ang chi chu stage hnih a lang chiang hle a, hei hi a chhan ber chu HNBR molecular chain decomposition temperature a inang lo group hrang hrang pahnih vang a ni. Stage hmasa ber chu butyl a ni ber
Stage hmasa ber chu butadiene-a double bond thermal cleavage vang a ni ber a, stage pahnihna chu heating process chhunga acrylonitrile chain segment cyclization avanga chelate compound siam a ni a, chu chu temperature sang takah chauh cleave theih a ni , chuvangin thermal cleavage stage langsar pahnih a awm a, rubber material decomposition temperature sang ber a lo lang a ni 468.49 °C , hei hian thermal stability sang tak a lantir a ni.
A tir lama thermal decomposition temperature (mass loss rate 5%) leh rubber material-a decomposition rate temperature sang ber chu a bul berah chuan trend inang an nei a, metal oxide dah belh hian rubber material-a mass loss rate sang ber a tihhniam thei a, chutah chuan zinc oxide rubber material hmun 5-a initial thermal decomposition temperature chu °C velin a tisang a ni material, which indicates that the 5 parts of zinc oxide can significantly blank rubber nena khaikhin chuan 15 improve the thermal stability of the rubber material, mahse zinc oxide dosage chu part 10 a nih chuan, a tir lama thermal decomposition Mahse, zinc oxide dosage chu part 10 a nih chuan a tir lama thermal decomposition temperature chu a tlahniam ta a ni. Hei hi: (1) zinc oxide a darh tha lo vang a ni thei; (2) peroxide vulcanization system-a zinc oxide tam lutuk chuan thermal stability tichhe thei cross-linking bonds a siam a. Hei hi a chhan dik tak chu chhui chian a la ni lo.A tir lama magnesium oxide rubber material-a part 5-a thermal decomposition temperature chu blank rubber material nena khaikhin chuan a tlahniam a, rubber material-a thermal decomposition temperature chu magnesium oxide zat chu part 10 a nih chauhvin tihsan theih a ni. Silicone rubber-a heat resistance characterize turin TG analysis hman a nih chuan, result-te chuan silicone rubber-a heat air aging performance leh oxygen atmosphere-a thermal decomposition temperature chu trend of change chu a inmil zawk tih a tarlang a, mahse he test-ah hian an pahnih hian correspondence engemaw tak an siam lo va, chu ai chuan maximum rate of mass loss leh trend of change in the performance of the hot air aging chu a inmil zawk a ni, chu chu a ni thei rubber chi hrang hrangte thermal decomposition leh thermal decomposition mechanism hrang hrang leh conditions (gas atmosphere ang chi) TG analysis vang a ni. Hei hi rubber chi hrang hrang thermal decomposition mechanism inang lo leh TG analysis (eg gas atmosphere) condition hrang hrang vang a ni thei a, chuvangin TG analysis hmanga rubber hot air aging resistance tehna atana hman a nih chuan a formulation tak tak leh test condition te chu uluk taka ngaihtuah a ngai a ni.
2. zinc oxide / magnesium oxide leh adhesives hman hian heat leh air aging resistance leh compression permanent deformation effect a tidanglam thei
Zinc oxide/magnesium oxide ratio chu 7/3 a nih chuan adhesive-a hot air aging performance-ah synergistic effect a awm a, adhesive hian heat resistance tha ber a nei a, magnesium oxide dah belh hian adhesive-a compression permanent deformation resistance-ah nghawng tha lo a nei thung.
Tawpna
(1) )HNBR peroxide vulcanization system-a zinc oxide emaw magnesium oxide emaw dah belh hian rubber material-ah activation effect a siam thei a, rubber material crosslinking degree a ti tha thei a, zinc oxide activity chu magnesium oxide aiin a sang zawk a, rubber material crosslinking degree hian a dose a san chuan upward trend a lantir a, mahse a zat a san chuan zinc oxide hi portion 10 a ni a, a dispersion tha lo avangin constant tensile stress a tlahniam thei a, mahse rubber material fluidity a chhe a, hei hian rebound value leh abrasion resistance ah nghawng a nei tlem hle. Abrasion resistance hian nghawng a nei tlem hle.
(2) Zinc oxide emaw magnesium oxide emaw vawi khat hman hian peroxide vulcanized HNBR compound-te heat leh air aging resistance nasa takin a ti ha thei a, chubakah heat resistance, heat resistance leh abrasion resistance a san chhoh zel chuan a ti ha thei bawk.
Heat resistance a sang a, zinc oxide dah belh hian rubber compression permanent deformation resistance a ti tha thei a, magnesium oxide erawh chuan a chungah nghawng a nei tlem hle thung.
(3)HNBR rubber thermal decomposition hi stage hnih a awm a, metal oxide dah belh hian mass loss rate sang ber a tihhniam thei a, zinc oxide hmun 5 vel hian rubber thermal stability nasa takin a ti tha thei a ni.
(4) Zinc oxide / magnesium oxide leh ratio 7 / 3 a nih chuan rubber hian heat resistance tha ber a nei a, mahse magnesium oxide hian rubber-in compression a do theihnaah nghawng tha lo tak a nei a, permanent deformation performance a nei bawk.