GA-2720
Herchy
| Availability: | |
|---|---|
| Gidaghanon: | |
Pagsulay: A/B ratio nga 1:1, 130°C x 5min x 15MPa
| Mga parameter sa produkto | |||||||
| produkto | GA-2720 | GA-2730 | GA-2740 | GA-2750 | GA-2760 | GA-2770 | |
| Panagway | Transparent | ||||||
| Lapot(Pa.s) |
2000 | 3000 | 3000 | 3500 |
4000 | 5000 |
|
| Katig-a (ShoreA) | 20 | 30 | 40 | 50 |
60 |
70 |
|
| Densidad (g/cm3) | 1.10 | 1.10 | 1.11 | 1.12 | 1.1.3 |
1.14 |
|
| Kusog sa Tensile (MPa) | 7.0 |
8.0 |
9.5 |
10.0 |
10.0 |
9.5 |
|
| Elongation(%) | 880 | 800 | 700 | 550 | 500 |
350 |
|
| Kusog sa luha (kN/m) | 16 | 30 | 35 |
40 | 35 |
30 |
|
| Linearshrinkage(%) | 2.1 | 2.1 | 2.1 | 2.0 | 2.0 |
2.0 |
|