GA- 11×3
Earcach
| Infhaighteacht: | |
|---|---|
| Cainníocht: | |
Tástáil: 1% den ghníomhaire leigheas (50% de ghreamú DBPMH i guma silicone), 175°C x 5min x 15MPa.
| Paraiméadair táirge | ||||||
| Táirge | GA- 1133 |
GA-1143 | GA- 1153 | GA-1163 | GA-1173 | GA-1183 |
| Dealramh | Tréshoilseach | |||||
| Williamplasticity |
115 |
150 |
205 |
240 |
280 |
310 |
| Cruas (ShoreA) |
30 |
40 |
50 |
60 |
70 |
80 |
| Dlús(g/cm3) | 1.10 |
1.12 |
1.16 |
1.19 |
1.22 |
1.22 |
| Neart teanntachta (MPa) |
7.5 |
7.5 |
9 |
8.5 |
8.5 |
7.5 |
| Fadú(%) | 700 |
500 |
450 |
400 |
300 |
200 |
| neart cuimilt (kN/m) | 16 |
20 |
20 |
20 |
20 |
16 |