Imikhiqizo ebunjiwe: imikhiqizo yenjoloba emincane nephakathi nendawo ebunjwa futhi ivuthwe ku-vulcanizer eyisicaba.


Uhlobo olufanayo lwezinkinga ezenzeka ekubunjweni kwenjoloba lubonakala emikhiqizweni ehlukene, njengokuthi: ukungabi khona kwenjoloba, ukuqhuma nokunye. Ngenxa yezinhlobo ezahlukene, amaqoqo kanye nemvelaphi yezinto zenjoloba, imishini nama-opharetha, ingahlaziywa kuphela ngesisekelo secala ngalinye.


1. L i-glue

Ukusebenza kwendawo (konke noma yendawo) okuxekethile, okumakiwe noma okungenalutho, izimbangela nezindlela zokuvimbela.

(1) Inani elinganele lezinto ezingeziwe Ukuqinisekisa ukuthi akukho ukushoda kweglue emgodini ngamunye, inani lempahla esetshenzisiwe kufanele linqunywe ngokunembile, lengezwe enanini eliphelele lezinto futhi liboniswe emibhalweni yenqubo.

(2) Ukucindezela okunganele, inani leglue alikwazi ukugcwalisa isikhunta sesikhunta, ingcindezi kufanele yandiswe ngendlela efanele.

(3) I-liquidity ye-adhesive impofu kakhulu. Uma ukusebenza komkhiqizo kuvumela, lungisa ifomula yerabha ukwandisa ipulasitiki. Khulisa ukucindezela noma sebenzisa ungqimba lwe-lubricant njenge-zinc stearate noma uwoyela we-silicone ebusweni besikhunta.

(4) Izinga lokushisa lesikhunta liphezulu kakhulu, futhi irabha ihangukile kancane futhi uketshezi luyancishiswa. Kufanele kube ezifanele ukunciphisa izinga lokushisa isikhunta lapho ulayisha, kodwa akufanele kube kakhulu, ngaphandle kwalokho izinga lokushisa isikhunta ngesikhathi esibekiwe ayikwazi ukukhuphukela lokushisa vulcanization futhi wenze yonke isikhunta enjoloba Scrap. Irabha ye-Silicone ingalayishwa ekushiseni okuphansi.

(5) Isikhathi esishisayo senjoloba sifushane kakhulu. Ifomula kufanele ithuthukiswe ukuze kuthuthukiswe ukumelana nokushisayo kwerabha.

(6) Ijubane lokulayisha nokuvala isikhunta lihamba kancane, libangela ukushisa nokushiswa, futhi indlela yokusebenza kufanele ithuthukiswe.

(7) Ukubekwa okungafanele kwesikhala kwenza irabha ingabi lula ukugcwalisa umgodi.

(8) Isakhiwo isikhunta ayinangqondo, futhi kuzokwenza injoloba akulula ukugcwalisa isikhunta imbobo ezifana: imikhiqizo ewumngcingo, kufanele lula isiqondiso ubude umkhiqizo kanye isiqondiso ingcindezi perpendicular.

(9) Ukucindezela kuyashesha kakhulu, irabha ikhishwa ngaphandle kwesikhunta ngaphambi kokugcwalisa umgodi, ukuze unqenqema olundizayo lujiye futhi umkhiqizo ungabi nezinto ezibonakalayo, isivinini sokucindezela kufanele sehliswe, futhi irabha igeleza kancane ingene emgodini ngaphansi kwengcindezi.


2. Ukuqhekeka komugqa we-buttress

Ukusebenza kwesikhunta ngemva kokuqalwa kwesikhunta ekuqhekekeni komkhiqizo, ngezinye izikhathi okundizayo okwenzeka emaphethelweni (okuvame ukwaziwa ngokuthi i-edge extraction), izimbangela nezindlela zokuvimbela.

(1) Ukucindezela okunganele noma ukushintshashintsha kwengcindezi Yenza ingcindezi yangaphakathi ye-raba cavity ngesikhathi senqubo ye-vulcanization inkulu kunokucindezela kwe-vulcanization. Futhi wenze isikhunta phezulu kancane, okubangela ukuqhekeka komkhiqizo, kufanele uhlole ingcindezi noma uhlole isizathu sokushintshashintsha kwengcindezi.

(2) Umfutho we-vulcanization mkhulu kakhulu. Injoloba icindezelwe kakhulu, lapho isikhunta sivulwa, ukucindezela kwehla kakhulu, umthamo wenjoloba ovuzayo ukhuphuka, enye ingxenye yomkhiqizo ivinjelwe isikhunta ayikwazi ukwanda, futhi isikhunta sikhululekile ukukhula emgqeni wesikhunta, ukucindezeleka kwangaphakathi okubangelwa ukunwetshwa okungalingani kuzoholela ekuqhekekeni komugqa, ingcindezi ye-vulcanization kufanele ibe yincane kakhulu futhi ivimbele isimo esifanelekile, ukuze kuvinjelwe ukuba kuncane kakhulu. Uma unqenqema olundizayo luqina ngemva kokwehliswa kwengcindezi, inani lezinto ezingeziwe lingancishiswa noma i-groove yokugeleza inganyuswa ngokufanele. (Phola ngaphansi kwengcindezi bese uphuma esikhunjeni).

(3) Ukushisa okuphezulu kwe-vulcanization kanye nesikhathi esifushane kubangela isizathu esiyinhloko semikhiqizo ewugqinsi, ngemva kokuvuthwa kwangaphandle kwemikhiqizo, ngenxa yokudluliswa kokushisa okuhamba kancane kwerabha, ingaphakathi lisasesimweni esingavulwanga, uma ingcindezi yehliswa ukuze iqale isikhunta, ukusabela kwangaphakathi kwe-vulcanization emdlalweni wezinto ezibonakalayo kuzochichima ngokushesha, futhi ngesikhathi esifanayo, ukwehla kwerabha, ngenxa yokushisa okuphelele. i-vulcanization yezinga lokuncipha kwerabha likhudlwana). Lezi zici ezimbili zenza unqenqema oluqhekekile emgqeni wesikhunta, kufanele lulungiswe kuzimo ze-vulcanization, kusetshenziswa izinga lokushisa eliphansi kanye nendlela ye-vulcanization yesikhathi eside noma indlela ye-vulcanization yokufudumala ngezigaba.

(4) Ukuxega kwendawo emgqeni wesikhunta kanye namandla amancane okubopha phakathi kwezinto zokunamathela yizizathu ezivamile zokuqhekeka kwendawo emgqeni wesikhunta. Kunezizathu eziningi zokuxega kwendawo, njengokuvaleka kwesikhunta okungekuhle, iglue eningi egeleza isuka esikhaleni, indlela engafanele yokukhipha impahla. Akucaci ukuthi kukhona ukuntuleka kweglue engxenyeni ethile yomugqa; isakhiwo sesikhunta asinangqondo (isiqondiso somugqa sihambisana nesiqondiso sokucindezela isakhiwo esivamile esingenangqondo, kufanele sigwenywe), i-glue inzima kakhulu, njll. Izinkinga ezithile kufanele zihlaziywe futhi zithuthukiswe.

(5) Ukucindezela kancane sekwephuze kakhulu. Uma ingaphezulu lerabha liye lavuvukala bese kuba nengcindezi encane, ngokuvamile yenza ipheya yemigqa iqhekeke.


3. I-Puffy, i-porous noma i-spongy

Izimbangela nezindlela zokuvimbela

(1) I-vulcanization akwanele. Izinga lokushisa liphansi kakhulu noma isikhathi sifushane kakhulu, ukuze ama-volatiles akhiqizwa yi-vulcanization angaqediwe ngokuhlanzekile, imbangela kufanele ikhonjwe futhi kuthathwe izinyathelo ezihambisanayo.

(2) Ukucindezela okunganele kwe-vulcanization, i-gas ne-vulcanization volatiles egcinwe emgodini wesikhunta ayikwazi ukukhishwa ngesikhathi, futhi ukucindezela kufanele kwandiswe ngendlela efanele.

(3) cindezela ngokushesha kakhulu, vala isikhunta ngokushesha, igesi ayikwazi ukukhishwa, kufanele icindezele kancane, ukuze isikhunta sivalwe kancane.

(4) Ukukhipha umoya okungalungile noma okungekho kwengcindezi ehamba kancane (okwaziwa ngokujwayelekile ngokuthi i-venting). Ukuze imikhiqizo eminingi idinga ukukhathala. Isikhathi, kusenesikhathi kakhulu noma sekwephuzile kakhulu kube ukukhathala okungafanelekile, kodwa futhi kuletha okunye okubi.

(5) Isakhiwo sesikhunta esingenangqondo Ngemikhiqizo yesakhiwo esiyinkimbinkimbi, kufanele isetshenziswe ngaphezulu kwesikhunta se-block, kusetshenziswa okunye okuvela ekuphunyukeni komthungo; izimbobo zomoya ezibonakala kalula zingengezwa ukuvula i-slot egijimayo yomoya, umgodi ongaphezulu wesifanekiso sodonga akufanele ujule kakhulu.

(6) Indlela yokulayisha engalungile, umoya osemgodini awukhishwe kalula. Ukuze isikhunta esinesakhiwo esiyinkimbinkimbi kanye neziphetho ezifile, izinto kufanele zisakazwe ngokulinganayo endaweni ngayinye ye-cavity lapho ifakwa esikhunjeni.

(7) Umoya nomswakama kuvaleleke kunjoloba. Lokhu kuvame ukubangelwa ukucwengwa kokushisa okungafanele noma ukugcinwa. Kufanele uthuthukise ikhwalithi yokucwenga okushisayo futhi ugcine irabha exubile kahle. Vala noma womise.

(8) izinga lokushisa eliphezulu le-vulcanization, i-vulcanization ngaphambi kwesikhathi kwendawo yenjoloba, ukuvimbela imvula yamahhala yomoya, umhwamuko kanye nezingxenye eziguquguqukayo erabha, ikakhulukazi irabha yemikhiqizo ewugqinsi. Izilinganiso ngo-2.(3)

(9) Ukulayisha okunganele Ngaphezu kokubangela ukuntuleka kweglue ebusweni bomkhiqizo, kungenza futhi ingaphakathi lingabi lukhuni futhi libe nezimbobo zomoya.

(10) Isivinini sokuvuthwa kwenjoloba sishesha kakhulu futhi ukuntengantenga kwangaphakathi akukwazi ukumiswa ukuze kuqine. Ifomula kufanele ilungiswe ukuze kuthuthukiswe isikhathi sokungeniswa kwerabha.


4. I-Delamination kanye nokuqhekeka

Izimbangela zokukhiqiza kanye nezindlela zokuvimbela

(1) ukubuyela kunjoloba (ngemuva kokuxuba impahla yenjoloba ayisetshenziswanga futhi ixubene nento entsha yenjoloba, le nto yenjoloba ibizwa ngokuthi ukubuyisela kurabha) kanye nokuxubana kwempahla yenjoloba lapho ukucwengisiswa kungafani, okuholela ezingeni elingahambisani le-vulcanization le- layering. Khulisa inani lokudlula elincanyana, uhlanganise ngokulinganayo.

(2) Irabha noma isikhunta singcoliswe amafutha nokunye ukungcola. Beka indawo engcolile, vikela irabha futhi uhlanze isikhunta.

(3) ngokufafaza isikhunta kakhulu ukukhululwa ejenti, ukuze ingxenye ukucwiliswa injoloba, okuholela imikhiqizo delamination, ngokuqhekeka, kancane ngangokunokwenzeka fafaza noma cha.

(4) Ukuxubana okungalingani noma ukufutha isithwathwa Ukufafaza isithwathwa kuyisenzo esibonakalayo se-agent ehlanganisa irabha (njenge-vulcanizing agent, antioxidant, plasticizer, njll.) ewa enjoloba. Irabha unvulcanized kanye injoloba vulcanized kungenzeka, iraba in isikhunta ngaphambi ukucwiliswa uma ungakwazi kahle ukuqeda mkhuba isifutho frost, izingxenye zomkhiqizo ayikwazi kahle kuhlanganiswe, futhi in the spray frost izingxenye ngokuqhekeka noma layering. Indlela yokuvimbela, ukuxuba ngokugcwele ngaphambi kokusetshenziswa, ayikwazi ukupakwa isikhathi eside kakhulu.

(5) Ipulasitiki yenjoloba imbi kakhulu. Ukucwenga ukushisa kwanele futhi i-vulcanization iphezulu ngangokunokwenzeka.


5. Ukubhidliza imifantu

Lesi sici sibhekisela ekudabukeni komkhiqizo ngesikhathi sokudilizwa, indawo edabukile iyahlukahluka ngenxa yezizathu ezihlukene zokudabuka, izimbangela nezindlela zokuvimbela zimi kanje.

(1) phezu kwesibabule ngenxa yokuthi imikhiqizo yesibabule ayiguquki ngokwanele, kulula ukubangela izinkinga zemishini lapho iphuma esikhunjini, ngokuvamile, ifaneleka ukunciphisa izinga lokushisa le-vulcanization ukuze unciphise isikhathi se-vulcanization, ingaxazulula izinkinga ezinjalo.

(2) Izinga lokushisa lesikhunta liphezulu kakhulu lapho lidilizwa Ama-molecule enjoloba asanyakaza ngobudlova, futhi lapho ehlangabezana nomoya obandayo, azopholiswa endaweni kuqala futhi enze ukucindezela kwangaphakathi ngengxenye endizayo yangemuva kokupholisa, okuzobangela kalula imifantu ebhidlizayo. Irabha ye-Silicone inamaphutha amaningi anjalo.

(3) Ukungasebenzisi i-ejenti yokukhulula noma inani le-ejenti yokukhulula akwanele

(4) Indlela yokuphuma kwesikhunta ayilungile futhi kufanele ithuthukiswe.

(5) Isakhiwo sesikhunta asinangqondo.

(6) Umgodi wokubumba awucutshungulwa kahle noma usetshenziswe isikhathi eside, okwandisa ubunzima bokuphuma kwesikhunta.

(7) Ukukhethwa kwempahla akunangqondo, kufanele kusetshenziswe amandla amahle okudabula, ukunwetshwa kwezinto zenjoloba, njenge-NR.


6. Futha isithwathwa

Imikhiqizo enengozi ifafaza isithwathwa, izimbangela zokukhiqiza kanye nezindlela zokuvimbela.

(1) I-vulcanization enganele, i-ejenti eyingozi kakhulu yokusabela okuphelele kanye nemvula yendawo yomkhiqizo.

(2) Inani lenhlanganisela ethile likhulu kakhulu, lidlula ukuncibilika kwenjoloba ene-vulcanized, ifomula kufanele ilungiswe.

(3) Ukuxutshwa kokungalingani kwenkomponi.

(4) Izinga lokushisa lokugcinwa komkhiqizo liphansi kakhulu, futhi ukuncibilika kwe-compound ku-rubber kuyancipha.


7. Ukuhlanekezela kanye nokuguqulwa

Izimbangela nezindlela zokuvimbela

(1) umnyango vulcanization akwanele, plasticity impahla, aphume isikhunta ngenxa amandla mechanical ukulenza ukuhlanekezela deformation, vulcanization akuyona imikhiqizo eyanele, emva vulcanization mkhuba ubuye sína, in the post-vulcanization inqubo kungase futhi kwenzeke deformation.

(2) i-vulcanization engalingani Okokuqala, umkhiqizo uminyene kakhulu, i-vulcanization engalingani ngaphakathi nangaphandle, ingaphakathi liyaqhubeka nokuvuvukala, ukuguqulwa komkhiqizo, izinyathelo ezifanayo njenge-2 (3). Okwesibili, izinga lokushisa lepuleti eliphezulu neliphansi alihambisani, okuholela ekuhlukeni kwezinga le-vulcanization yezingxenye ezihlukahlukene zemikhiqizo ehlanjululwe, okubangela ukubola.

(3) ngaphandle kwezinga lokushisa lesikhunta liphezulu kakhulu iraba isenayo ipulasitiki enkulu, kulula ukuyishintsha ngaphansi kwesenzo samandla emishini, ene-5 (2)

(4) Ngemikhiqizo enezingxenye zensimbi, usayizi wezingxenye zensimbi awufaneleki. Nakuba irabha ingafakwa emgodini wesikhunta nokunwebeka kwayo, ibuyela esimweni sayo sasekuqaleni ngokushesha ngemva kokushiya isikhunta, okuholela ekuguquguqukeni kwawo wonke umkhiqizo.

(5) Imikhiqizo enendwangu eboshiwe Ngoba izinga lokuncipha kwendwangu kanye ne-adhesive lihlukile. Ukuguqulwa ngenxa yokuncipha kokungalingani ngemva kokupholisa isikhunta.

(6) odongeni ukushuba umehluko, ukupholisa isivinini shrinkage akufani, kulula ukwenza udonga mncane ingxenye deformation deflection. Imikhiqizo yensimbi irabha ehlanzekile ingxenye encane ephuma esikhunjeni nayo kulula ukubangela ukubola. Ukupholisa okulungisiwe.

(7) Ukuvikelwa nokulondolozwa okungafanele.


IZIXHUMANISI EZISHESHAYO

IMIKHIQIZO YETHU

ULWAZI LOKUXHUMANA

Engeza: No.33, Lane 159, Taiye Road, Fengxian District, Shanghai
Ucingo / WhatsApp / Skype: +86 15221953351
I-imeyili:  info@herchyrubber.com
Copyright     2023 Shanghai Herchy Rubber Co., Ltd. Imephu yesayithi |   Inqubomgomo Yobumfihlo | Sekela Ngu I-Leadong.