Tel: +86 15221953351 E-mail hmanga zawhfiah theih a ni. info@herchyrubber.com
Please Choose Your Language

SOLUTIONS THIL AWM DAN

You are here: In » A chinfel dan tur » A chinfel dan tur » Rubber molding atana quality lama harsatna awm fo leh a chinfel dan

Rubber molding atana quality lama harsatna awm fo leh solution

Moulded products: chu rubber product tenau leh lian lo, flat vulcanizer-a molded leh vulcanized a ni.


Rubber molding-a harsatna chi khat lo awm chu thil chi hrang hrangah a lang chhuak a, chungte chu: rubber tlakchhamna, bulging leh a dangte a ni. Rubber material chi hrang hrang, batch hrang hrang leh origin hrang hrang, machine leh operator te avang hian case-by-case basis chauhvin a zirchiang thei a ni.


1. loGlue a awm

Performance of the surface (all or local) loose, pockmarked or hollow, a chhan leh a ven dan.

(1) Thil dah belh tlem Cavity tinah glue tlakchhamna a awm loh nan, thil hman zat dik taka hriat a ngai a, thil awm zawng zawngah dah belh tur a ni a, process documentation-ah a lang tur a ni.

(2) Pressure tling lo, glue tam lutuk hian mold cavity a luah khat thei lo a, pressure chu a dik taka tihsan tur a ni.

(3) Adhesive liquidity a chhe lutuk. Product performance a phal chuan plasticity tihpun nan rubber formula chu siamrem tur a ni. Pressure tihsan emaw, mold chung lamah zinc stearate emaw silicone oil ang chi lubricant layer hmangin hnawih rawh.

(4) Mould temperature a sang lutuk a, rubber chu a then a kang a, fluidity a tlahniam bawk. Load laiin mould temperature tihhniam a rem tur a ni a, mahse a tam lutuk tur a ni lo, chutiang a nih loh chuan hun bituk chhunga mold temperature chu vulcanization temperature-ah a sang thei lo va, mold pumpui chu rubber scrap-ah a siam thei lo. Silicone rubber hi temperature hniam zawkah load theih a ni.

(5) Rubber scorching time hi a tawi lutuk. Rubber-a scorching resistance tihchak nan formula hi siam that tur a ni.

(6) Mould load leh khar speed a slow lutuk a, a kang leh a kang a, operation technique pawh siam that a ngai.

(7) Blank dah dik loh chuan rubber chu a khuh chu a luah khat awlsam lo hle.

(8) Mold structure chu a dik lo a, chubakah rubber chu mold cavity fill awlsam lo turin a siam ang hetiang ang: product te tak te tan chuan product sei lam hawi leh pressure perpendicular lam hawi a ti awlsam tur a ni.

(9) Pressurization a rang lutuk a, rubber chu cavity a khat hmain mold atang chuan extrude chhuah a ni a, chutiang chuan flying edge chu a thick a, product ah material a tlachham a, pressurization speed chu a hniam tur a ni a, pressure hnuaiah rubber chu cavity chhungah zawi zawiin a luang lut a ni.


2. Buttress line a crack chhuak

Product cracking-a mold-a start-up hnua mold performance, a chang chuan flying edge shrinkage phenomenon (edge ​​extraction tia hriat lar), a chhan leh a ven dan.

(1) Pressure tling lo emaw pressure inthlak danglam emaw Vulcanization process chhunga rubber cavity chhungril pressure chu vulcanization pressure aiin a tam zawk turin siam rawh. Tin, mold chu tlem a sang zawka siam la, product cracking thlentu, pressure check emaw pressure fluctuation reason check emaw tur a ni.

(2) Vulcanization pressure a lian lutuk. Rubber chu nasa takin a compress a, mold hawn a nih chuan pressure a tlahniam nasa hle a, vulcanized rubber volume a sang a, product hmun dang chu mold vangin a khap a, a zau thei lo a, mold chu mold line-ah a zalen a, a zau lo vanga internal stress chuan line chu a ti chhe ang a, vulcanization pressure chu a remchan dan anga siam tur a ni, a ven theih nan.. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. .. lian lutuk leh te lutuk. Pressure tihhniam hnua flying edge a thick chuan material dah zat tihtlem theih a ni a, a remchan dan angin flow groove pawh tihpun theih a ni bawk. (Pressure hnuaiah a lum la, mold atang chuan chhuak rawh).

(3) Vulcanization temperature sang leh hun rei lote chhunga thil thick siam chhan ber a ni a, pawn lam atanga vulcanization a nih hnuah, rubber-a heat transfer slow vangin, a chhung lam chu unvulcanized state-ah a la awm a, mold start turin pressure tihhniam a nih chuan, material play-a internal vulcanization reaction chu rang takin a overflow ang a, chutih rual chuan, temperature tlahniam vangin, rubber chu shrinkage hi a na hle (rubber vulcanization kimchang nen khaikhin chuan shrinkage rate a lian zawk). Heng thil pahnih hian mold line-a cracked edge chu a siam a, vulcanization condition-ah siamrem tur a ni a, low temperature leh long time vulcanization method emaw phased warming vulcanization method emaw hmangin.

(4) Mould line-a local looseness leh adhesive materials inkara bonding strength tlem te hi mold line-a local cracking awm chhan tlangpui a ni. Local looseness chhan tam tak a awm a, chu chu mold closing tha lo, gap atanga glue luang tam lutuk, material release dan dik lo te hi a ni. Line hmun khatah glue tlakchhamna a awm tih a chiang lo; mold structure chu a dik lo (line kalna chu pressure lam hawia parallel a nih chuan typical unreasonable structure a ni a, pumpelh tur a ni), glue a khauh lutuk, etc. Harsatna bikte chu thlirlet a, siam that a ngai.

(5) Pressure slow tlai lutuk. Rubber chunglam chu vulcanized a nih a, chutah slow pressure a nih chuan line pahnih chu cracked tir fo ang che.


3. Puffy, porous emaw spongy emaw

A chhan leh inven dan tur

(1) Vulcanization hi a tawk lo. Temperature a hniam lutuk emaw, hun a tawi lutuk emaw a nih avangin vulcanization atanga volatile lo chhuak te chu thianghlim taka tihbo a nih loh avangin a chhan hriatchhuah a, a inmil tur ruahmanna siam a ngai a ni.

(2) Vulcanization pressure tling lo, mold cavity-a gas leh vulcanization volatile awmte chu a hun takah a chhuak thei lo va, pressure chu a remchan dan anga tihsan tur a ni.

(3) pressure rang lutuk, mold khar vat, gas chu a chhuak thei lo, zawi zawiin pressurized tur a ni a, chutiang chuan mold chu zawi zawiin a khar ang.

(4) Slow pressure (venting tia hriat lar) venting dik lo emaw, venting awm lo emaw. Product tam zawk tan chuan exhaust a ngai. Timing, hma lutuk emaw tlai lutuk emaw chu exhaust dik lo a ni a, mahse thil tha lo dang pawh a rawn keng tel bawk.

(5) unreasonable mold structure Complex structure products atan chuan block mold tam zawk hman tur a ni a, mold seam escape atanga dang hman tur a ni easy to appear air holes dah belh theih a ni a, air running slot hawn theih a ni a, upper template wall cavity chu a thuk lutuk tur a ni lo.

(6) Loading dan dik lo, cavity chhunga boruak chu awlsam takin a chhuak lo. Complex structure leh dead ends nei mold tan chuan material chu mold chhunga dah a nih hunah cavity awmna hmun tinah inang tlang taka sem darh tur a ni.

(7) Rubber chhungah hian boruak leh tuihna a tang a. Hei hi heat refining emaw storage dik lo vang a ni tlangpui. Hot refining quality i ti tha tur a ni a, mixed rubber chu i vawng tha tur a ni. Seal emaw dry emaw rawh.

(8) vulcanization temperature sang, rubber chunglam vulcanization hma, rubber chhunga boruak, tui vapor leh volatile components, a bik takin thick products rubber free precipitation awm lohna. A tehnate chu 2.(3) .

(9) Loading tling lo Product chung lamah glue a awm loh bakah a chhung lam a dense lo thei a, air holes a nei thei bawk.

(10) Rubber vulcanization speed a chak lutuk a, a chhunga volatiles te chu harden turin precipitate theih a ni lo. Rubber induction period tha zawk nan formula hi siamrem tur a ni.


4. Delamination leh cracking te

Production chhan leh ven dan tur

. Thin pass zat tipung la, a rualin mix rawh.

(2) Rubber emaw mold emaw chu grease leh bawlhhlawh dangin a ti bawlhhlawh a ni. A bawlhhlawh lai chu layer la, rubber chu humhim la, mold cavity chu tifai rawh.

(3) mold release agent tam lutuk spray, chutiang chuan rubber-a immersion thenkhat, a rah chhuah products delamination, cracking, a tlem thei ang bera spray emaw spray loh emaw.

(4) Frost inhmeh lo taka inhmeh emaw, spray emaw Spraying frost hi rubber atanga rubber compounding agent (vulcanizing agent, antioxidant, plasticizer, etc. ang chi) lo chhuak taksa lama thil thleng a ni. Unvulcanized rubber leh vulcanized rubber a awm thei a, immersion hmaa mold-a rubber awm chuan spray frost phenomenon chu i tihbo tha thei lo a, product-a parts te chu a inzawm tha thei lo a, spray frost-ah chuan parts cracking emaw layering emaw a awm thei bawk. Preventing method, hman hmaa fully mixing, rei lutuk park theih loh.

(5) Rubber plasticity a chhe lutuk. Heat refining a tawk a, vulcanization pawh a sang thei ang bera tih a ni.


5. Crack awmte demoulding

He defect hian demolding process-a product tearing tihna a ni a, tearing area hi a tear chhan hrang hrang avangin a danglam a, a chhan leh a ven dan pawh a hnuaia mi ang hian a ni.

(1) over sulphur a chhan chu over sulfur products hi a flexible tawk lo a, mold atanga a chhuah hunah mechanical strain siam awlsam, a tlangpuiin, vulcanization temperature tihhniamna tur vulcanization hun tawi zawka siam a remchang, chutiang harsatna chu a chinfel theih

(2) Demoulding laiin mould temperature a sang lutuk Rubber molecule te hi nasa takin an la kal a, boruak lum an tawn chuan local-ah an lum hmasa ang a, post-cooling flying part nen internal pressure an siam ang a, chu chuan awlsam takin demoulding crack a siam ang. Silicone rubber hian chutiang chhiatna chu a nei tam zawk.

(3) Release agent hman loh emaw, release agent zat emaw a tawk lo

(4) Mold chhuah dan hi a dik lo a, siam that a ngai.

(5) Mould structure hi a dik lo.

(6) Mold cavity hi process tha lo emaw, hun rei tak hman emaw a nih avangin mold chhuah harsatna a tizual a ni.

(7) Material thlan chu a dik lo a, tear strength tha tak, rubber material elongation, NR ang chi te hman tur a ni.


6. Frost (frost) hmanga spray thin ang che

Vulcanized products spray frost, a siam chhuah chhan leh a ven dan te.

(1) Vulcanization tling lo, product surface-a reaction kimchang leh precipitation atana vulcanizing agent tam zawk.

(2) Compound engemaw zat a tam lutuk a, vulcanized rubber solubility aia tam a nih chuan formula chu siamrem tur a ni.

(3) Compound chu a inhmeh lo hle.

(4) Product dahna temperature a hniam lutuk a, rubber chhunga compound awm solubility a tlahniam bawk.


7. Distortion leh deformation

A chhan leh inven dan tur

(1) vulcanization department a tawk lo a, material plasticity, mold atanga chhuak chu mechanical force vangin distortion deformation a siam a, vulcanization chu product a tling lo a, vulcanization phenomenon pawh a na zawk hnuah, post-vulcanization process-ah pawh deformation a thleng thei bawk.

(2) uneven vulcanization Pakhatnaah chuan product chu a thick lutuk a, a chhung leh pawnah uneven vulcanization, a chhung lam chu a vulcanize chhunzawm zel a, product deformation, 2 (3)-a tehna ang chiah a ni. Pahnihnaah chuan, plate chung leh hnuai lam temperature a inmil lo va, chu chuan vulcanized products hmun hrang hrang vulcanization degree a inang lo va, deformation a thlen a ni.

(3) out of the mold temperature a sang lutuk rubber hian plasticity lian tak a la nei a, mechanical forces action hnuaia deformation awlsam tak, 5 (2) .

(4) Metal part nei product tan chuan metal parts size hi a qualify lo. Rubber hi a elasticity nen mold cavity-ah dah theih ni mah se, mold a chhuahsan hnuah a dinhmun hmasaah a kir leh nghal a, chu chuan a thil siam zawng zawng chu a tichhe vek a ni.

(5) Clamped fabric nei products A chhan chu fabric leh adhesive te shrinkage rate a inang lo. Mould atanga a lum chhuah hnua a shrinkage inang lo avanga deformation.

(6) wall thickness danglamna, cooling shrinkage speed a inang lo, a awlsam zawngin thin wall part of the deflection deformation siam. Metal products pure rubber thin part out of the mould pawh hi deformation siam awlsam tak a ni. Cooling tihfel a ni.

(7) Hriselna leh humhalh dan dik lo.


QUICK LINKS A AWM VE ANG

CONTACT THIL AWM DAN

Add: No.33, Lane 159, Taiye kawngpui, Fengxian District, Shanghai-a awm a ni
Tel / WhatsApp / Skype: +86 15221953351 ah zawhfiah theih a ni
E-mail hmangin:  info@herchyrubber.com