FV9600
Herchy
beskikberens: | |
---|---|
kwantiteit: | |
Items | Yndeks | ||
Klasse | FV9660 | FV9670 | |
Ferskining Testmethoden | Wyt | ||
Spesifike swiertekrêft / G / CM3 | ASTM D792 | 1.46 | 1.48 |
Hardness / Shorea | ASTM D2240 | 60 | 70 |
Tensile sterkte / MPA | ASTM D412 | 6.8 | 6.5 |
ELONGATION BY BREAK /% | ASTM D412 | 310 | 290 |
Trienter sterkte / kn / m | ASTM D624-B | 17 | 17 |
* Heat wjerstân | Hardheid feroarje / wâl a | +5 | +5 |
Tensile Sterkte feroaring,% | 3.8 | 3.5 | |
Tensile Sterkte feroaring,% | 161 | 154 | |
IRM903 | ASTM D471 | 5.5 | 5.2 |
Fuel C | ASTM D471 | 20 | 20 |
Flame-retardant nivo | GBT10707-2008 | FV 0 | FV 0 |
Genêzen tastân | Foegje 0.7 dielen fan BIS tafoegje (2 + 5), ien etappe Vulcanisaasje 170 ℃ × 15min, twa poadiumfaske, 200 ℃ × 4h. |
Items | Yndeks | ||
Klasse | FV9660 | FV9670 | |
Ferskining Testmethoden | Wyt | ||
Spesifike swiertekrêft / G / CM3 | ASTM D792 | 1.46 | 1.48 |
Hardness / Shorea | ASTM D2240 | 60 | 70 |
Tensile sterkte / MPA | ASTM D412 | 6.8 | 6.5 |
ELONGATION BY BREAK /% | ASTM D412 | 310 | 290 |
Trienter sterkte / kn / m | ASTM D624-B | 17 | 17 |
* Heat wjerstân | Hardheid feroarje / wâl a | +5 | +5 |
Tensile Sterkte feroaring,% | 3.8 | 3.5 | |
Tensile Sterkte feroaring,% | 161 | 154 | |
IRM903 | ASTM D471 | 5.5 | 5.2 |
Fuel C | ASTM D471 | 20 | 20 |
Flame-retardant nivo | GBT10707-2008 | FV 0 | FV 0 |
Genêzen tastân | Foegje 0.7 dielen fan BIS tafoegje (2 + 5), ien etappe Vulcanisaasje 170 ℃ × 15min, twa poadiumfaske, 200 ℃ × 4h. |