GA-11 × 3
Herchy
| Saadavus: | |
|---|---|
| Kogus: | |
Test: 1% kõvendit (50% DBPMH pasta silikoonkummis), 175 °C x 5 min x 15 MPa.
| Toote parameetrid | ||||||
| Toode | GA-1133 |
GA-1143 | GA-1153 | GA-1163 | GA-1173 | GA-1183 |
| Välimus | Läbipaistev | |||||
| Williamplastilisus |
115 |
150 |
205 |
240 |
280 |
310 |
| Kõvadus (ShoreA) |
30 |
40 |
50 |
60 |
70 |
80 |
| Tihedus (g/cm3) | 1.10 |
1.12 |
1.16 |
1.19 |
1.22 |
1.22 |
| Tõmbetugevus (MPa) |
7.5 |
7.5 |
9 |
8.5 |
8.5 |
7.5 |
| pikenemine (%) | 700 |
500 |
450 |
400 |
300 |
200 |
| Rebenemistugevus (kN/m) | 16 |
20 |
20 |
20 |
20 |
16 |